CO catalyst as well as preparation method and application thereof
The preparation of CO catalysts through multi-step drying and calcining processes has solved the problems of insufficient low-temperature catalytic performance and narrow window temperature in the prior art, and achieved efficient CO catalytic oxidation, enhancing the stability and efficiency of the catalyst.
Patent Information
- Application Number
- CN202410959760.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The catalytic performance of existing CO catalysts under low temperature conditions is insufficient, the window temperature is narrow, and the active ingredients are prone to fall off, resulting in a large difference in pressure drops between the front and back of the catalyst bed, increasing energy consumption.
The CO catalyst is prepared by a multi-step drying and calcining process, including stale decomposition at 10-35°C, multiple drying and gradual heating and calcining, and the catalyst clay composed of support such as copper oxide, cobalt oxide, manganese oxide and titanium dioxide are added to make pores. agents, binders and structural enhancers optimize the microstructure and properties of the catalyst.
The catalytic activity of CO catalyst at low temperatures is improved, the window temperature is widened, the stability and efficiency of the catalyst are enhanced, and energy consumption is reduced.
Smart Images

Figure BDA0004949934600000141 
Figure BDA0004949934600000161 
Figure BDA0004949934600000171
Abstract
Description
Technical Field
[0001] The invention relates to a CO catalyst and a preparation method and application thereof. Background Art
[0002] CO is not easy to react chemically in the air, has stable properties, and can stay in the atmosphere for a long time. When the CO in the air exceeds a certain value, it may cause human poisoning, hypoxia, and even endanger life. In addition, CO is flammable and explosive, and can easily cause an explosion. Catalytic oxidation is a major method for removing CO.
[0003] CN114950469A discloses a carbon monoxide catalyst, which is prepared from raw materials including a carrier, an active component precursor, a pore expander and a binder; wherein the carrier includes titanium dioxide, aluminum oxide, manganese dioxide and a porous carrier, and the porous carrier is selected from one or more of diatomaceous earth or bentonite; the active component includes a copper oxide precursor, a manganese oxide precursor, a cobalt oxide precursor and a cerium oxide precursor. The catalytic performance of the carbon monoxide catalyst at low temperatures needs to be improved.
[0004] CN114570435A discloses a method for preparing a honeycomb catalyst, which comprises mixing a catalyst powder containing active ingredients with a binder and a dispersant to form a mixture, adding water to form an impregnation liquid; and repeatedly subjecting an acid-treated ceramic honeycomb carrier to the steps of impregnation, drying, and calcination in the impregnation liquid to obtain a honeycomb catalyst. The active ingredients are mainly manganese oxide and copper oxide, and other metal oxides are auxiliary ingredients. Other metal oxides include any one or more of cerium oxide, tin oxide, cobalt oxide, lanthanum oxide, praseodymium oxide, samarium oxide, europium oxide, gadolinium oxide, potassium oxide, calcium oxide, zinc oxide, magnesium oxide, and nickel oxide. This method loads the active ingredients on the carrier, and the active ingredients are easy to fall off, which also leads to a large difference in pressure drop before and after the catalyst bed, increasing energy consumption.
[0005] CN109513447A discloses a method for preparing a carbon monoxide removal catalyst, wherein a titanium dioxide precursor and an activated alumina are fully mixed in a preset ratio, and after mixing, manganese oxide, a copper oxide precursor, a ferric oxide precursor, a silicon dioxide, a cerium oxide precursor, a tin oxide precursor, a magnesium oxide precursor, a niobium pentoxide precursor and an antimony pentoxide precursor are added in a preset ratio, and fully kneaded; a pore expander, a lubricant, a mold release agent and deionized water are added to continue fitting, and the catalyst precursor is extruded on a mold to obtain a catalyst precursor; the catalyst precursor is dried and calcined to obtain a carbon monoxide removal catalyst. The window temperature and catalytic efficiency of the catalyst need to be improved. Summary of the invention
[0006] In view of this, an object of the present invention is to provide a method for preparing a CO catalyst, which can improve the catalytic activity of the CO catalyst under low temperature conditions. Furthermore, the catalyst obtained by the preparation method has a wider window temperature. Another object of the present invention is to provide a CO catalyst. Another object of the present invention is to provide a use of a CO catalyst.
[0007] The above purpose is achieved through the following technical solutions.
[0008] In one aspect, the present invention provides a method for preparing a CO catalyst, comprising the following steps:
[0009] (1) aging the catalyst sludge at a temperature of 10 to 35° C. and a humidity of 60 to 95% for 15 to 35 hours to obtain aged sludge;
[0010] (2) forming the aged mud material into a honeycomb catalyst body;
[0011] (3) drying the honeycomb catalyst body at a temperature of 10 to 30° C. to obtain a primary dried body;
[0012] The primary dried green body is secondary dried at a temperature of 20 to 45° C. to obtain a secondary dried green body;
[0013] Drying the secondary dried green body for a third time at a temperature of 40 to 60° C. to obtain a tertiary dried green body;
[0014] Drying the thrice-dried green body a fourth time at a temperature of 55 to 75° C. to obtain a quadruple-dried green body;
[0015] Drying the quadruple dried green body for a fifth time at a temperature of 70 to 90° C. to obtain a five-time dried green body;
[0016] Drying the five-time dried green body six times at a temperature of 85-110° C. to obtain a six-time dried green body;
[0017] Drying the green body after six dryings for seven times at a temperature of 95 to 125° C. to obtain a dried green body;
[0018] (4) calcining the dried body at 150-350° C. for the first time and then calcining it at 300-600° C. for the second time to obtain a CO catalyst;
[0019] The catalyst slurry comprises a carrier, a manganese oxide precursor, a pore former, a binder, a lubricant and a structural enhancer;
[0020] The carrier is selected from one or more of copper oxide, cobalt oxide, titanium dioxide, manganese dioxide, cerium oxide, and aluminum oxide; the pore-forming agent is selected from one or more of starch, wood chips, activated carbon, and polymethyl methacrylate; the lubricant is selected from one or more of glycerol, salad oil, and ethanolamine; the structural reinforcing agent is selected from one or more of glass fiber and pulp fiber; and the binder is selected from one or more of carboxymethyl cellulose, polyethylene glycol, and aluminum sol.
[0021] According to the preparation method of the present invention, preferably, the pH of the catalyst sludge is 6.5-9, and the water content is 20-40 wt%.
[0022] According to the preparation method of the present invention, preferably, the amount of the carrier is 500-850 parts by weight, the amount of the manganese oxide precursor is 60-100 parts by weight, the amount of the pore former is 5-60 parts by weight, the amount of the structural enhancer is 80-120 parts by weight, the amount of the binder is 10-50 parts by weight, and the amount of the lubricant is 5-15 parts by weight.
[0023] According to the preparation method of the present invention, preferably, the carrier is selected from the following compositions:
[0024] (a) Copper oxide, manganese dioxide and titanium dioxide;
[0025] (b) Copper oxide, manganese dioxide and cobalt oxide;
[0026] (c) Copper oxide, cerium oxide, aluminum oxide and cobalt oxide.
[0027] According to the preparation method of the present invention, preferably, drying is carried out under the condition of humidity of 60-95%; the first drying time is 15-36 hours, the second drying time is 15-36 hours, the third drying time is 15-36 hours, the fourth drying time is 15-36 hours, the fifth drying time is 15-36 hours, the sixth drying time is 15-36 hours, and the seventh drying time is 15-36 hours.
[0028] According to the preparation method of the present invention, preferably, the first drying temperature is less than the second drying temperature, less than the third drying temperature, less than the fourth drying temperature, less than the fifth drying temperature, less than the sixth drying temperature, less than the seventh drying temperature.
[0029] According to the preparation method of the present invention, preferably, in step (2), the stale mud material is extruded into shape using a screw extruder at an extrusion speed of 0.1 to 0.8 m / min;
[0030] The heating rate from the initial temperature to the primary calcination temperature is 2-10°C / min, and the primary calcination time is 0.5-3h;
[0031] The heating rate from the primary calcination temperature to the secondary calcination temperature is 0.3 - 5 °C / min, and the secondary calcination time is 2 - 7 h.
[0032] According to the preparation method of the present invention, preferably, it includes the following steps:
[0033] Mix the carrier and the pore-forming agent for 5 - 20 min to obtain a first mixture; mix the first mixture and the structure enhancer for 30 - 70 min to obtain a second mixture; mix the second mixture and the binder for 10 - 40 min to obtain a third mixture; mix the third mixture and the manganese oxide precursor for 10 - 40 min to obtain a fourth mixture; mix the fourth mixture and the lubricant for 5 - 20 min to obtain the catalyst paste.
[0034] On the other hand, the present invention provides a CO catalyst obtained by the preparation method described in any one of claims 1 - 8.
[0035] On yet another aspect, the present invention provides the use of the above CO catalyst in the catalytic oxidation of CO.
[0036] The CO catalyst prepared by the method of the present invention has high catalytic activity at low temperatures. Further, the CO catalyst has a wide window temperature. Detailed Embodiments
[0037] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0038] <Preparation Method of CO Catalyst>
[0039] The preparation method of the CO catalyst of the present invention includes the following steps: (1) the aging step; (2) the shaping step; (3) the drying step; and (4) the calcination step. In some embodiments, it further includes the step of forming the catalyst paste.
[0040] The old steps
[0041] The present invention ages the catalyst paste to obtain an aged paste.
[0042] The catalyst paste includes a carrier, a manganese oxide precursor, a pore-forming agent, a binder, a structure enhancer, and a lubricant. The catalyst paste may further include water and / or a pH regulator. In some embodiments, the catalyst paste consists only of the above raw materials.
[0043] The carrier is selected from one or more of copper oxide, cobalt oxide, titanium dioxide, manganese dioxide, cerium oxide and aluminum oxide. The amount of the carrier can be 500 to 850 parts by weight. In some embodiments, the amount of the carrier is 600 to 750 parts by weight. In other embodiments, the amount of the carrier is 700 to 720 parts by weight.
[0044] In certain embodiments, the carrier includes copper oxide, manganese dioxide and titanium dioxide. The amount of copper oxide can be 80 to 120 parts by weight; preferably 90 to 110 parts by weight; more preferably 100 to 105 parts by weight. The amount of manganese dioxide can be 150 to 250 parts by weight; preferably 180 to 220 parts by weight; more preferably 200 to 210 parts by weight. The amount of titanium dioxide can be 350 to 450 parts by weight; preferably 370 to 430 parts by weight; more preferably 400 to 410 parts by weight.
[0045] In other embodiments, the carrier includes copper oxide, manganese dioxide and cobalt oxide. The amount of copper oxide can be 80 to 120 parts by weight; preferably 90 to 110 parts by weight; more preferably 100 to 105 parts by weight. The amount of manganese dioxide can be 150 to 250 parts by weight; preferably 180 to 220 parts by weight; more preferably 200 to 210 parts by weight. The amount of cobalt oxide can be 400 to 500 parts by weight; preferably 420 to 480 parts by weight; more preferably 450 to 460 parts by weight.
[0046] In some further embodiments, the carrier includes copper oxide, cerium oxide, aluminum oxide and cobalt oxide. The amount of copper oxide can be 80 to 120 parts by weight; preferably 90 to 110 parts by weight; more preferably 100 to 105 parts by weight. The amount of cerium oxide can be 10 to 100 parts by weight; preferably 30 to 80 parts by weight; more preferably 50 to 60 parts by weight. The amount of aluminum oxide can be 10 to 100 parts by weight; preferably 30 to 80 parts by weight; more preferably 50 to 60 parts by weight. The amount of cobalt oxide can be 350 to 450 parts by weight; preferably 370 to 430 parts by weight; more preferably 400 to 410 parts by weight.
[0047] The carrier can be used in the form of a powder. The carrier raw material can be dried and then ball-milled in a ball mill to form a carrier powder.
[0048] The carrier can improve the catalytic performance of the CO catalyst at low temperatures and widen the window temperature.
[0049] The manganese oxide precursor may be a water-soluble inorganic manganese salt. According to one embodiment of the present invention, the manganese oxide precursor is manganese nitrate. The amount of the manganese oxide precursor may be 60 to 100 parts by weight; preferably 60 to 80 parts by weight; more preferably 70 to 80 parts by weight. This can improve the catalytic performance of the CO catalyst at low temperatures and widen the window temperature.
[0050] The pore former can be selected from one or more of starch, activated carbon, sawdust, and polymethyl methacrylate. In some embodiments, the pore former is starch. In other embodiments, the pore former is activated carbon. In still other embodiments, the pore former is sawdust. The amount of the pore former can be 5 to 60 parts by weight. In some embodiments, the amount of the pore former is 8 to 15 parts by weight. In other embodiments, the amount of the pore former is 35 to 45 parts by weight. In this way, appropriate pores can be formed in the catalyst, the catalytic performance of the catalyst at low temperatures can be improved, and the window temperature can be widened.
[0051] The structural reinforcing agent can be selected from one or more of glass fiber and pulp fiber. In some embodiments, the structural reinforcing agent is glass fiber. In other embodiments, the structural reinforcing agent is pulp fiber. The amount of the structural reinforcing agent can be 80 to 120 parts by weight; preferably 90 to 110 parts by weight; more preferably 100 to 105 parts by weight.
[0052] The binder can be selected from one or more of carboxymethyl cellulose, aluminum sol, and polyethylene glycol. In some embodiments, the binder is carboxymethyl cellulose. In other embodiments, the binder is aluminum sol. In still other embodiments, the binder is polyethylene glycol. The amount of the binder can be 10 to 50 parts by weight. In some embodiments, the amount of the binder is 15 to 22 parts by weight. In other embodiments, the amount of the binder is 28 to 33 parts by weight.
[0053] The lubricant may be selected from one or more of glycerol, salad oil, and ethanolamine. In some embodiments, the lubricant is glycerol. In other embodiments, the lubricant is ethanolamine. In still other embodiments, the lubricant is glycerol and salad oil. The mass ratio of glycerol to salad oil may be (0.5-2):1; preferably (0.8-1.8):1; more preferably (1.2-1.6):1.
[0054] The amount of lubricant used may be 5 to 15 parts by weight, preferably 8 to 14 parts by weight, and more preferably 10 to 12 parts by weight.
[0055] The pH of the catalyst sludge may be 6.5 to 9, preferably 7 to 8.5, and more preferably 7.5 to 8. The catalyst sludge may be adjusted to the above pH by adding a pH adjuster. The pH adjuster may be an alkaline pH adjuster. Preferably, the pH adjuster is aqueous ammonia.
[0056] The water content of the catalyst sludge can be 20-40wt%; preferably 25-35wt%; more preferably 27-30wt%. The water content is determined according to the following method: (1) Dry the weighing bottle at 105°C for 2h, take it out, let it cool, cover it with a cap and weigh it on an analytical balance with an accuracy of 1 / 10,000 until constant weight is reached (the difference between two weighings does not exceed 0.0005g), and record the mass of the weighing bottle as A, in g. (2) Take about 5.0g of the catalyst sludge and put it into the weighing bottle, record the total mass of the catalyst sludge and the weighing bottle as B, in g; open the bottle cap of the weighing bottle, dry the weighing bottle and the catalyst sludge in a 105°C forced air drying oven (WGL-30T, Tianjin Test Instrument Co., Ltd.), take it out after drying for 4h each time, let it cool, cover it with a cap and weigh it until constant weight is reached, and record the mass of the dried catalyst sludge and the total mass of the weighing bottle as C. Calculated according to the formula: moisture content = (BC) / (BA)×100%.
[0057] Under the above pH and humidity conditions, the plasticity of the catalyst slurry can be improved, the defects of the catalyst body can be reduced, and the catalytic performance of the catalyst can be improved.
[0058] The aging temperature may be 10 to 35°C; preferably 15 to 30°C; more preferably 20 to 25°C.
[0059] The aging can be carried out at a humidity of 60 to 95%, preferably 70 to 90%, and more preferably 75 to 80%.
[0060] The aging time may be 15 to 35 hours, preferably 20 to 30 hours, and more preferably 24 to 28 hours.
[0061] The catalyst sludge can be sealed with plastic wrap and then aged.
[0062] Forming steps
[0063] The invention shapes the aged mud material to obtain a honeycomb catalyst blank.
[0064] The aged mud material can be extruded and formed by a screw extruder to form a honeycomb catalyst body. The extrusion speed can be 0.1 to 0.8 m / min, preferably 0.3 to 0.5 m / min. The cross section of the catalyst body can be in the positive direction.
[0065] The aged mud material can be filtered and squeezed in a mud kneading machine before forming. The filtering and squeezing can be performed at a temperature below 50°C. The filtering and squeezing can be performed multiple times. For example, 2 to 5 times; or 2 to 3 times.
[0066] Drying steps
[0067] The present invention dries the honeycomb catalyst blank once to obtain a primary dried blank; dries the primary dried blank twice to obtain a secondary dried blank; dries the secondary dried blank thrice to obtain a thrice dried blank; dries the thrice dried blank four times to obtain a quadruple dried blank; dries the quadruple dried blank five times to obtain a quintuple dried blank; dries the quintuple dried blank six times to obtain a sixth dried blank; and dries the sixth dried blank seven times to obtain a dried blank.
[0068] The primary drying temperature is 10 to 30°C, preferably 15 to 25°C, and more preferably 20 to 22°C.
[0069] The primary drying time may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0070] The secondary drying temperature is 20 to 45°C, preferably 25 to 40°C, and more preferably 30 to 35°C.
[0071] The secondary drying time may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0072] The tertiary drying temperature is 40-60°C, preferably 45-55°C, and preferably 50-52°C.
[0073] The three drying times may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0074] The fourth drying temperature is 55 to 75°C, preferably 60 to 70°C, and more preferably 65 to 68°C.
[0075] The fourth drying time may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0076] The fifth drying temperature is 70 to 90°C, preferably 75 to 85°C, and more preferably 80 to 82°C.
[0077] The five drying times may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0078] The sixth drying temperature is 85 to 110°C, preferably 90 to 100°C, and more preferably 95 to 97°C.
[0079] The sixth drying time may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0080] The seventh drying temperature is 95 to 125°C, preferably 105 to 120°C, and more preferably 110 to 115°C.
[0081] The seventh drying time may be 15 to 36 hours, preferably 20 to 30 hours, and more preferably 24 to 26 hours.
[0082] In the present invention, the primary drying temperature < the secondary drying temperature < the tertiary drying temperature < the fourth drying temperature < the fifth drying temperature < the sixth drying temperature < the seventh drying temperature.
[0083] Drying can be performed at a humidity of 60 to 95%, preferably 70 to 90%, and more preferably 80 to 85%.
[0084] The above drying conditions are helpful to fully dry the catalyst body without affecting the morphology of the catalyst body, thereby improving the catalytic performance of the catalyst and widening the window temperature.
[0085] Roasting steps
[0086] The present invention performs a primary calcination on the dried green body and then performs a secondary calcination to obtain a CO catalyst. After the secondary calcination, natural cooling can be performed.
[0087] The primary calcination temperature is 150-350°C, preferably 200-300°C, and more preferably 250-270°C.
[0088] The primary calcination time may be 0.5 to 3 hours, preferably 0.8 to 2 hours, and more preferably 1 to 1.5 hours.
[0089] The heating rate from the initial temperature to the primary calcination temperature may be 2 to 10°C / min, preferably 3 to 8°C / min, and more preferably 5 to 6°C / min.
[0090] The secondary calcination temperature is 300-600°C; preferably 400-500°C; more preferably 450-470°C
[0091] The secondary roasting time may be 2 to 7 hours, preferably 3 to 6 hours, and more preferably 4 to 5 hours.
[0092] The heating rate from the primary calcination temperature to the secondary calcination temperature may be 0.3 to 5°C / min, preferably 1 to 4°C / min, and more preferably 2 to 3°C / min.
[0093] Steps for forming catalyst sludge
[0094] The present invention forms a catalyst mud from raw materials.
[0095] In some embodiments, the method includes the following steps:
[0096] Mix the carrier and the pore-forming agent for 5 to 20 minutes; preferably 10 to 15 minutes, to obtain a first mixture.
[0097] Mix the first mixture and the structure enhancer for 30 to 70 minutes; preferably 40 to 60 minutes, to obtain a second mixture. The structure enhancer can be added to the first mixture in multiple portions.
[0098] Mix the second mixture and the binder for 10 to 40 minutes; preferably 15 to 30 minutes, to obtain a third mixture.
[0099] Mix the third mixture and the manganese oxide precursor for 10 to 40 minutes; preferably 15 to 30 minutes, to obtain a fourth mixture. The manganese oxide precursor can be used in the form of an aqueous solution.
[0100] Mix the fourth mixture and the lubricant for 5 to 20 minutes; preferably 10 to 15 minutes, to obtain the catalyst mud.
[0101] <CO Catalyst and Its Use>
[0102] The CO catalyst of the present invention is prepared by the above preparation method. The catalyst of the present invention has a high catalytic oxidation efficiency for CO. Therefore, the present invention provides the use of the above catalyst in the catalytic oxidation of CO. CO can be present in flue gas. The catalytic oxidation temperature can be 50 to 400 °C; preferably 60 to 150 °C; more preferably 100 to 130 °C.
[0103] The concentration of CO in the flue gas can be 5000 to 18000 ppm; preferably 8000 to 15000 ppm; more preferably 10000 to 12000 ppm.
[0104] The concentration of NO in the flue gas can be 100 to 500 ppm; preferably 200 to 400 ppm; more preferably 300 to 350 ppm.
[0105] The concentration of SO 2 in the flue gas can be less than or equal to 800 ppm. In some embodiments, it is 300 to 700 ppm; preferably 400 to 600 ppm.
[0106] The content of water vapor in the flue gas can be 2 to 25 vol%; preferably 5 to 20 vol%; more preferably 10 to 12 vol%.
[0107] CO in the flue gas 2The content of may be 2 to 30 vol%, preferably 5 to 20 vol%, and more preferably 15 to 17 vol%.
[0108] O in flue gas 2 The content of may be 5 to 30 vol%, preferably 10 to 20 vol%, and more preferably 15 to 17 vol%.
[0109] NO in flue gas 2 The concentration can be 5 to 50 ppm; preferably 10 to 40 ppm; more preferably 20 to 30 ppm.
[0110] Examples 1 to 3
[0111] (1) The carrier is dried at 110°C to obtain a dry carrier. The dry carrier is ball-milled in a ball mill to obtain carrier powder; the ball-to-material ratio is 2:1, and the rotation speed is 250 r / min; during the ball milling process, the ball mill is rotated forward for 8 minutes, then reversed for 8 minutes, and then rested for 3 minutes, and the above rotation procedure is repeated 10 times.
[0112] Place the carrier powder in a mixing device, add a pore-forming agent to the mixing device, mix for 10 minutes, and obtain a first mixture. Add a structural enhancer to the first mixture in batches, mix for 50 minutes, and obtain a second mixture. Add a binder to the second mixture, mix for 20 minutes, and obtain a third mixture. Add an aqueous solution of manganese nitrate to the third mixture, mix for 20 minutes, and obtain a fourth mixture. Add a lubricant to the fourth mixture, mix for 10 minutes, and obtain a catalyst sludge. During the mixing process, ammonia water is used to adjust the pH of the catalyst sludge so that the pH of the catalyst sludge is 7.5-8. The water content of the catalyst sludge is 27-30wt%.
[0113] The catalyst mud was sealed with a plastic wrap; then aged for 24 hours at a temperature of 20° C. and a humidity of 80% to obtain aged mud.
[0114] (2) The aged mud is filtered and extruded in a mud kneader at a temperature below 50°C, and then extruded in a screw extruder to obtain a honeycomb catalyst body with 18×18 holes. The extrusion speed is 0.3-0.5 m / min.
[0115] (3) The honeycomb catalyst blank is dried at a temperature of 20°C and a humidity of 80% for 24 hours to obtain a first dried blank. The first dried blank is dried at a temperature of 35°C and a humidity of 80% for 24 hours to obtain a second dried blank. The second dried blank is dried at a temperature of 50°C and a humidity of 80% for 24 hours to obtain a third dried blank. The third dried blank is dried at a temperature of 65°C and a humidity of 80% for 24 hours to obtain a fourth dried blank. The fourth dried blank is dried at a temperature of 80°C and a humidity of 80% for 24 hours to obtain a fifth dried blank. The fifth dried blank is dried at a temperature of 95°C and a humidity of 80% for 24 hours to obtain a sixth dried blank. The sixth dried blank is dried at a temperature of 110°C and a humidity of 80% for 24 hours to obtain a dried blank.
[0116] (4) The dried green body was placed in a calcination device, calcined at 250°C for 1 hour, then calcined at 450°C for 4 hours, and cooled naturally to obtain a CO catalyst. The heating rate from the initial temperature to 250°C was 5°C / min, and the heating rate from 250°C to 450°C was 2°C / min.
[0117] The types and amounts of raw materials are shown in Table 1.
[0118] Table 1
[0119]
[0120] Comparative Example 1
[0121] Except that step (3) is different from that in Example 1, the rest is the same as that in Example 1. Step (3) is specifically as follows:
[0122] The honeycomb catalyst body was dried at a temperature of 20°C and a humidity of 80% for 48 hours to obtain a first dried body. The first dried body was dried at a temperature of 35°C and a humidity of 80% for 48 hours to obtain a second dried body. The second dried body was dried at a temperature of 50°C and a humidity of 80% for 48 hours to obtain a third dried body. The third dried body was dried at a temperature of 65°C and a humidity of 80% for 24 hours to obtain a fourth dried body.
[0123] Comparative Example 2
[0124] Except that step (3) is different from that in Example 1, the rest is the same as that in Example 1. Step (3) is specifically as follows:
[0125] The honeycomb catalyst blank is dried at a temperature of 20°C and a humidity of 80% for 24 hours to obtain a first dried blank. The first dried blank is dried at a temperature of 35°C and a humidity of 80% for 24 hours to obtain a second dried blank. The second dried blank is dried at a temperature of 50°C and a humidity of 80% for 24 hours to obtain a third dried blank. The third dried blank is dried at a temperature of 65°C and a humidity of 80% for 24 hours to obtain a fourth dried blank. The fourth dried blank is dried at a temperature of 95°C and a humidity of 80% for 48 hours to obtain a fifth dried blank. The fifth dried blank is dried at a temperature of 110°C and a humidity of 80% for 24 hours to obtain a dried blank.
[0126] Comparative Example 3
[0127] Except that the sixth drying temperature is 120° C. and the seventh drying temperature is 135° C., the rest is the same as in Example 1. Step (3) of this comparative example is as follows:
[0128] The honeycomb catalyst blank is dried for 24 hours at a temperature of 20°C and a humidity of 80% to obtain a first dried blank. The first dried blank is dried for 24 hours at a temperature of 35°C and a humidity of 80% to obtain a second dried blank. The second dried blank is dried for 24 hours at a temperature of 50°C and a humidity of 80% to obtain a third dried blank. The third dried blank is dried for 24 hours at a temperature of 65°C and a humidity of 80% to obtain a fourth dried blank. The fourth dried blank is dried for 24 hours at a temperature of 80°C and a humidity of 80% to obtain a fifth dried blank. The fifth dried blank is dried for 24 hours at a temperature of 120°C and a humidity of 80% to obtain a sixth dried blank. The sixth dried blank is dried for 24 hours at a temperature of 135°C and a humidity of 80% to obtain a dried blank.
[0129] Experimental example
[0130] The CO catalyst was placed in a fixed bed quartz tube reactor, and the test gases with different compositions were tested at different temperatures. The space velocity was 20000h -1 , the test time is 2800min. After the test time, the CO concentration in the catalytic gas is detected, and the CO conversion rate is calculated according to the following formula:
[0131]
[0132] Wherein, η represents CO conversion rate, %; C 1 Indicates the CO concentration in the gas to be tested, mg / Nm 3 ; C 2Indicates the CO concentration in the gas after catalysis, mg / Nm 3 .
[0133] Table 2 Gas composition to be tested
[0134] Gas composition Gas to be tested 1 Gas to be tested 2 Gas to be tested 3 Gas to be tested 4 <![CDATA[NO(mg / Nm 3 )]]> 300 300 300 300 <![CDATA[NO 2 (mg / Nm 3 )]]> 20 20 20 20 <![CDATA[SO 2 (mg / Nm 3 )]]> 0 0 0 500 <![CDATA[CO(mg / Nm 3 )]]> 10000 10000 10000 10000 <![CDATA[CO 2 (%)]]> 15 20 15 15 <![CDATA[O 2 (%)]]> 16 16 16 16 <![CDATA[H 2 O(%)]]> 10 10 20 20
[0135] Table 3CO conversion rate (%)
[0136]
[0137] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing a CO catalyst, characterized in that: The steps include: (1) aging the catalyst sludge at a temperature of 10 to 35° C. and a humidity of 60 to 95% for 15 to 35 hours to obtain aged sludge; (2) forming the aged mud material into a honeycomb catalyst body; (3) drying the honeycomb catalyst body at a temperature of 10 to 30° C. to obtain a primary dried body; The primary dried green body is secondary dried at a temperature of 20 to 45° C. to obtain a secondary dried green body; Drying the secondary dried green body for a third time at a temperature of 40 to 60° C. to obtain a tertiary dried green body; Drying the thrice-dried green body a fourth time at a temperature of 55 to 75° C. to obtain a quadruple-dried green body; Drying the quadruple dried green body for a fifth time at a temperature of 70 to 90° C. to obtain a five-time dried green body; Drying the five-time dried green body six times at a temperature of 85-110° C. to obtain a six-time dried green body; Drying the green body after six dryings for seven times at a temperature of 95 to 125° C. to obtain a dried green body; (4) calcining the dried body at 150-350° C. for the first time and then calcining it at 300-600° C. for the second time to obtain a CO catalyst; The catalyst slurry comprises a carrier, a manganese oxide precursor, a pore former, a binder, a lubricant and a structural enhancer; The carrier is selected from one or more of copper oxide, cobalt oxide, titanium dioxide, manganese dioxide, cerium oxide, and aluminum oxide; the pore-forming agent is selected from one or more of starch, wood chips, activated carbon, and polymethyl methacrylate; the lubricant is selected from one or more of glycerol, salad oil, and ethanolamine; the structural reinforcing agent is selected from one or more of glass fiber and pulp fiber; and the binder is selected from one or more of carboxymethyl cellulose, polyethylene glycol, and aluminum sol.
2. The preparation method according to claim 1, characterized in that: The catalyst sludge has a pH of 6.5 to 9 and a water content of 20 to 40 wt%.
3. The preparation method according to claim 1, characterized in that: The carrier is used in an amount of 500 to 850 parts by weight, the manganese oxide precursor is used in an amount of 60 to 100 parts by weight, the pore former is used in an amount of 5 to 60 parts by weight, the structure reinforcing agent is used in an amount of 80 to 120 parts by weight, the binder is used in an amount of 10 to 50 parts by weight, and the lubricant is used in an amount of 5 to 15 parts by weight.
4. The preparation method according to claim 1, characterized in that: The carrier is selected from one of the following composition: (a) Copper oxide, manganese dioxide and titanium dioxide; (b) Copper oxide, manganese dioxide and cobalt oxide; (c) Copper oxide, cerium oxide, aluminum oxide and cobalt oxide.
5. The preparation method according to claim 1, characterized in that: Drying is carried out under the condition of humidity of 60-95%; the first drying time is 15-36 hours, the second drying time is 15-36 hours, the third drying time is 15-36 hours, the fourth drying time is 15-36 hours, the fifth drying time is 15-36 hours, the sixth drying time is 15-36 hours, and the seventh drying time is 15-36 hours.
6. The preparation method according to claim 1, characterized in that: The first drying temperature is less than the second drying temperature, less than the third drying temperature, less than the fourth drying temperature, less than the fifth drying temperature, less than the sixth drying temperature, less than the seventh drying temperature.
7. The preparation method according to claim 1, characterized in that: Step (2) using a screw extruder to extrude the stale mud material into a shape at an extrusion speed of 0.1 to 0.8 m / min; The heating rate from the initial temperature to the primary calcination temperature is 2-10°C / min, and the primary calcination time is 0.5-3h; The heating rate from the primary roasting temperature to the secondary roasting temperature is 0.3-5°C / min, and the secondary roasting time is 2-7h.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The steps include: The carrier and the pore-forming agent are mixed for 5 to 20 minutes to obtain a first mixture; the first mixture and the structural reinforcing agent are mixed for 30 to 70 minutes to obtain a second mixture; the second mixture and the binder are mixed for 10 to 40 minutes to obtain a third mixture; the third mixture and the manganese oxide precursor are mixed for 10 to 40 minutes to obtain a fourth mixture; the fourth mixture and the lubricant are mixed for 5 to 20 minutes to obtain a catalyst slurry.
9. A CO catalyst, characterized in that The CO catalyst is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the CO catalyst according to claim 9 in CO catalytic oxidation.
Citation Information
Patent Citations
De-carbon monoxide catalyst and preparation method thereof
CN109513447A
Honeycomb catalyst as well as preparation method and application thereof
CN114570435A
Carbon monoxide catalyst as well as preparation method and application thereof
CN114950469A
Low temperature CO oxidation non-noble metal catalyst
CN101143321A
Preparation process of honeycomb SCR (selective catalytic reduction) denitration catalyst