Preparation method and application of nano metal oxide catalyst

The preparation of nanometal oxide catalysts by hydrothermal reaction in industrial wastewater has solved the problem of high viscosity of heavy oil, achieved efficient viscosity reduction of heavy oil and reuse of environmentally friendly resources, and reduced mining costs.

CN118904353AActive Publication Date: 2024-11-08SOUTHWEST PETROLEUM UNIV

Patent Information

Application Number
CN202410969329.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The high viscosity of heavy oil leads to poor liquidity, the investment cost or low efficiency of existing technology mining methods, and the metal ions of industrial wastewater cannot be effectively recycled, affecting environmental protection and resource reuse.

Method used

By hydrothermal reaction between iron salt and sodium hydroxide in industrial wastewater, a nanometal oxide catalyst is prepared and combined with an oil-soluble modifier to form regular nanoparticles for hydrothermal cracking of heavy oil Catalytic viscosity reduction.

Benefits of technology

It achieves efficient viscosity reduction effect of heavy oil, maintains stable catalyst performance, has the advantages of environmental protection and resource reuse, is easy to operate and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904353A_ABST
    Figure CN118904353A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of crude oil catalysis, in particular to a preparation method and application of a nano metal oxide catalyst, and the preparation method comprises the following steps: A, dissolving ferric salt in wastewater to obtain a ferric salt solution, dissolving sodium hydroxide in wastewater to obtain a sodium hydroxide solution, then dropwise adding the ferric salt solution into the sodium hydroxide solution, and uniformly mixing to obtain a mixed solution; a mixed solution is obtained; b, carrying out hydrothermal reaction on the mixed solution in the step A, centrifuging the reacted substance, collecting the precipitate, washing and drying to obtain a nano metal oxide catalyst precursor; and C, adding the nano metal oxide catalyst precursor in the step B into an oil-soluble modifier, centrifuging after reaction, collecting precipitate, and drying to obtain the nano metal oxide catalyst. The method is used for reducing the viscosity of the thickened oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crude oil catalysis, and in particular to a preparation method and application of a nano metal oxide catalyst. Background Art

[0002] With the rapid growth of oil consumption, conventional oil supply is gradually in short supply. Heavy oil (API gravity <22, viscosity>100mPa·s) is an unconventional oil, but it has excellent development prospects, and heavy oil accounts for about 70% of the total oil reserves. If heavy oil can be effectively utilized, the problem of oil resource shortage can be effectively solved. The problem is that heavy oil has a high viscosity, which leads to its poor fluidity, making it a huge problem in its exploitation that needs to be solved urgently. In the past few decades, people have conducted in-depth research on various ways to improve the fluidity of heavy oil. The main methods for heavy oil exploitation are physical methods (such as thermal oil recovery, steam stimulation method), chemical methods (fire burning oil layer method, active water viscosity reduction method), among which thermal recovery is the main method to reduce the viscosity of heavy oil during exploitation, but its investment cost is high. In recent years, chemical modification and viscosity reduction methods have made great progress. Catalysts and hydrogen donors are added to the reservoir, and heavy oil undergoes hydrothermal cracking under high temperature, high pressure and catalyst action. During the reaction, the catalyst can effectively promote the decomposition of long molecular chains into free radical fragments, some of which are quenched to form shorter molecules, and others are copolymerized. The former reaction is conducive to viscosity reduction, while the latter reaction is not conducive to viscosity reduction. The addition of hydrogen donors provides a large number of hydrogen radicals, which can help quench the free radical fragments produced by hydrothermal cracking and inhibit their copolymerization, thereby increasing the viscosity reduction rate. Heavy oil hydrothermal cracking catalysts can be roughly divided into mineral type, water-soluble catalysts, oil-soluble catalysts, amphiphilic catalysts and dispersed multiphase catalysts according to their properties.

[0003] Industrial wastewater contains a lot of metal ions, which will cause serious harm to the environment if discharged directly, but the metal ions can still be recycled and used to synthesize heavy oil viscosity reduction catalysts. This has a very important research significance for recycling wastewater and synthesizing heavy oil viscosity reduction catalysts. Summary of the invention

[0004] In order to solve the above technical problems, an embodiment of the present invention provides a preparation method and application of a nano metal oxide catalyst.

[0005] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:

[0006] In one aspect, the present invention provides a method for preparing a nano metal oxide catalyst, comprising the following steps:

[0007] A. dissolving iron salt in waste water to obtain an iron salt solution, dissolving sodium hydroxide in waste water to obtain a sodium hydroxide solution, and then adding the iron salt solution dropwise to the sodium hydroxide solution to mix well to obtain a mixed solution;

[0008] B. subjecting the mixed solution of step A to a hydrothermal reaction, centrifuging the reacted material, collecting the precipitate, washing and drying it to obtain a nano-metal oxide catalyst precursor;

[0009] C. Add the nano metal oxide catalyst precursor in step B to the oil-soluble modifier, centrifuge after the reaction, collect the precipitate, and dry to obtain the nano metal oxide catalyst.

[0010] In some embodiments, in step A, the iron salt includes at least one of ferric chloride hexahydrate, ferric nitrate nonahydrate and ferric sulfate.

[0011] In some embodiments, in step A, the mass ratio of the iron salt to the wastewater is (0.01-0.05):1.

[0012] In some embodiments, in step A, the molar ratio of sodium hydroxide to iron salt is 3:1.

[0013] In some embodiments, in step B, the temperature of the hydrothermal reaction is 140°C to 200°C.

[0014] In some embodiments, in step B, the hydrothermal reaction time is 6 to 16 hours.

[0015] In some embodiments, in step C, the oil-soluble modifier is oleic acid or oleylamine.

[0016] In some embodiments, in step C, the mass ratio of the oil-soluble modifier to the nano metal oxide catalyst precursor is 1:1 to 3:1.

[0017] On the other hand, the present invention provides an application of a nano metal oxide catalyst prepared by the above preparation method in reducing the viscosity of heavy oil.

[0018] Compared with the prior art, the present invention has at least the following beneficial effects:

[0019] (1) The present invention uses industrial wastewater as solvent, iron salt and sodium hydroxide to synthesize nano metal oxides through a hydrothermal method. The size of the nano metal oxides prepared by the present invention can reach 50nm, with a narrow size distribution and a regular polygonal shape. The nano particles have excellent activity in the hydrothermal cracking and modification of heavy oil, and the regular morphology enables the catalyst performance to be kept stable during the catalytic reaction, so that the catalyst always maintains high catalytic activity. The nano metal oxides prepared by the present invention are applied to heavy oil viscosity reduction and have excellent viscosity reduction effect.

[0020] (2) The present invention uses industrial wastewater containing metal ions to prepare nano metal oxides, and recycles the wastewater, which is of great significance for environmental protection, resource recycling, and reduction of economic losses, and the operation is convenient and controllable. In addition, the nano metal oxide prepared by the present invention has Fe2O3 as the main component and contains SiO2, CaO, MgO, MnO and other components. Compared with the existing nano Fe2O3, it has a smaller particle size and a more regular morphology, thereby improving its catalytic activity in hydrothermal reforming of heavy oil.

[0021] (3) The preparation method of the present invention is simple, and only requires generating nano metal oxides by a hydrothermal method, and then performing a step of modification and drying. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is the X-ray diffraction pattern of the nano metal oxide obtained in Comparative Example 1;

[0023] Figure 2 The SEM image of the nano-metal oxide obtained in Comparative Example 1 is shown in FIG.

[0024] Figure 3 is a particle size distribution diagram of the nano metal oxide obtained in Comparative Example 1;

[0025] Figure 4 is the X-ray diffraction pattern of the nano metal oxide obtained in Comparative Example 2;

[0026] Figure 5 This is the SEM image of the nano-metal oxide obtained in Comparative Example 2;

[0027] Figure 6 is the X-ray diffraction pattern of the nano metal oxide obtained in Example 1;

[0028] Figure 7 is the X-ray diffraction pattern of the nano metal oxide obtained in Example 2;

[0029] Figure 8 This is the SEM image of the commercial iron oxide in Comparative Example 1. DETAILED DESCRIPTION

[0030] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.

[0031] In one aspect, the present invention provides a method for preparing a nano metal oxide catalyst, comprising the following steps:

[0032] A. Dissolving iron salt in waste water to obtain an iron salt solution, dissolving sodium hydroxide in waste water to obtain a sodium hydroxide solution, and then adding the iron salt solution dropwise to the sodium hydroxide solution to mix well to obtain a mixed solution, wherein the waste water is industrial waste water containing calcium, silicon, magnesium, manganese, iron and other ions;

[0033] B. subjecting the mixed solution of step A to a hydrothermal reaction, centrifuging the reacted material, collecting the precipitate, washing and drying it to obtain a nano-metal oxide catalyst precursor;

[0034] C. Add the nano metal oxide catalyst precursor in step B to the oil-soluble modifier, centrifuge after the reaction, collect the precipitate, and dry to obtain the nano metal oxide catalyst.

[0035] In some embodiments, in step A, the iron salt includes at least one of ferric chloride hexahydrate, ferric nitrate nonahydrate and ferric sulfate.

[0036] In some embodiments, in step A, the mass ratio of the iron salt to the wastewater is (0.01-0.05):1, illustratively, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1 or 0.05:1.

[0037] In some embodiments, in step A, the molar ratio of sodium hydroxide to iron salt is 3:1.

[0038] In some embodiments, in step B, the temperature of the hydrothermal reaction is 140°C to 200°C, and illustratively, it can be 140°C, 160°C, 180°C, or 200°C.

[0039] In some embodiments, in step B, the hydrothermal reaction time is 6 to 16 hours, and illustratively, it can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, or 16 hours.

[0040] In some embodiments, in step C, the oil-soluble modifier is oleic acid or oleylamine.

[0041] In some embodiments, in step C, the mass ratio of the oil-soluble modifier to the nano metal oxide catalyst precursor is 1:1 to 3:1, and illustratively, it can be 1:1, 2:1 or 3:1.

[0042] On the other hand, the present invention provides an application of a nano metal oxide catalyst prepared by the above preparation method in reducing the viscosity of heavy oil.

[0043] Specifically, heavy oil is placed in a reactor, water is added at an oil-water ratio of 1:1, and a nano metal oxide catalyst is added to the reactor, hydrothermal catalytic cracking is carried out at a certain temperature, the reaction is carried out for a certain time, and then the oil sample after the reaction is taken out to measure the viscosity and SARA; in the present invention, the hydrothermal catalytic cracking reaction is carried out at 180-260°C (for example, 180°C, 200°C, 220°C, 240°C, 260°C) for 8-24h (for example, 8h, 12h, 16h, 20h, 24h); in the present invention, the mass ratio of the nano metal oxide catalyst to the heavy oil is 0.005:1.

[0044] The invention uses industrial waste water as solvent, iron salt and sodium hydroxide, and synthesizes nano metal oxides by a hydrothermal method. The size of the nano metal oxides prepared by the invention can reach 50nm, the size distribution is narrow, and the nano metal oxides are in a regular polygonal shape. The nano metal oxides prepared by the invention are applied to heavy oil viscosity reduction and have excellent viscosity reduction effect.

[0045] Example 1

[0046] Take industrial wastewater, the composition of which is shown in Table 1. Dissolve 1gFeCl3·6H2O and 0.45gNaOH in 20mL of wastewater respectively. After complete dissolution, mix and stir the two evenly, then add them to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and place the hydrothermal reactor in an oven to react at 160°C for 12h. Collect the precipitate of the reacted substance at a speed of 12500r / min with a centrifuge, wash it with pure water several times, and then place the solid in an oven and dry it at 60°C for 12h. The obtained powder is the nano-metal oxide catalyst precursor. Dissolve 0.07g oleic acid in 30mL methanol, add 0.07g of the nano-metal oxide catalyst precursor obtained in the above steps, stir at room temperature for 1h, collect the precipitate of the reacted substance at a speed of 12500r / min with a centrifuge, and place the obtained precipitate in a vacuum drying oven and dry it at 60°C for 12h to obtain a nano-metal oxide catalyst. The components of the nano metal oxide catalyst are: 93.6wt% of Fe2O3, 1.5wt% of CaO, 0.9wt% of SiO2, 0.8wt% of MgO, 0.3wt% of MnO, and the remainder is organic matter and inevitable impurities that are difficult to detect.

[0047] Example 2

[0048] Take industrial wastewater, the main components of which are shown in Table 1. Dissolve 1gFeCl3·6H2O and 0.45gNaOH in 20mL of wastewater respectively. Mix the two after they are completely dissolved, and then add them to a stainless steel hydrothermal reactor lined with polytetrafluoroethylene. Place the hydrothermal reactor in an oven and react at 160°C for 12h. Collect the precipitate of the reacted substance with a centrifuge at a speed of 12500r / min, wash it with pure water several times, and then place the solid in an oven and dry it at 60°C for 12h. The obtained powder is the nano-metal oxide catalyst precursor. Dissolve 0.07g of oleylamine in 30ml of methanol, add 0.07g of the nano-metal oxide catalyst precursor obtained in the above steps, stir at room temperature for 1h, collect the precipitate of the reacted substance with a centrifuge at a speed of 12500r / min, place the obtained precipitate in a vacuum drying oven, and dry it at 60°C for 12h to obtain a nano-metal oxide catalyst. The components of the nano metal oxide catalyst are: 92.8wt% of Fe2O3; 1.6wt% of CaO; 0.8wt% of SiO2; 0.6wt% of MgO; 0.2wt% of MnO; and the remainder is organic matter and inevitable impurities that are difficult to detect.

[0049] The X-ray diffraction pattern of the nano-metal oxide catalyst obtained in Example 2 is as follows: Figure 7 As shown in the figure, the 2θ peaks are located at 24.1°, 33.1°, 35.6°, 40.8°, 49.4°, 54.1°, 57.6°, 62.4° and 64.0°, respectively, belonging to (012), (104), (110), (113), (024), (116), (018), (214) and (300) crystal planes, respectively, and the synthesis is a nano metal oxide catalyst with α-Fe2O3 as the main component. However, compared with the X-ray diffraction patterns of Comparative Examples 1 and 2, the peak intensity is significantly weakened, and a carbon-related peak appears at 26.0°, proving that oleylamine has effectively modified the nano metal oxide catalyst.

[0050] Comparative Example 1

[0051] Take industrial wastewater, the main components of which are shown in Table 1. Dissolve 1gFeCl3·6H2O and 0.45gNaOH in 20mL of wastewater respectively. After they are completely dissolved, mix and stir them evenly. Then add them into a stainless steel hydrothermal reactor lined with polytetrafluoroethylene. Place the hydrothermal reactor in an oven and react at 160°C for 12h. Collect the precipitate of the reacted substance with a centrifuge at a speed of 12500r / min, wash it with pure water several times, and then place the solid in an oven and dry it at 60°C for 12h. The obtained powder is a nano metal oxide catalyst. The components of the nano metal oxide catalyst are: Fe2O3 is 94wt%; CaO is 1.6wt%; SiO2 is 1.1wt%; MgO is 0.6wt%; MnO is 0.4wt%; and the remainder is unavoidable impurities.

[0052] The X-ray diffraction pattern of the nano metal oxide catalyst obtained in this comparative example 1 is as follows Figure 1 As shown, the 2θ peaks are located at 24.1°, 33.1°, 35.6°, 40.8°, 49.4°, 54.1°, 57.6°, 62.4° and 64.0°, respectively, belonging to the (012), (104), (110), (113), (024), (116), (018), (214) and (300) crystal planes, respectively, and the synthesis is a nano-metal oxide catalyst with α-Fe2O3 as the main component. The SEM image of the nano-metal oxide catalyst synthesized in this comparative example 1 is as follows Figure 2 As shown, from Figure 2 It can be seen that most of the nanoparticles are regular polyhedrons, and a small number are spherical. Figure 3 It can be seen that the particle size distribution is narrow, mainly concentrated between 30 and 60 nm.

[0053] Comparative Example 2

[0054] Take industrial wastewater, the composition of which is shown in Table 1, dissolve 1g FeCl3·6H2O and 0.45g NaOH in 20mL wastewater respectively, mix and stir the two after they are completely dissolved, and then add them into a stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and place the hydrothermal reactor in an oven to react at 200°C for 12h. Collect the precipitate of the reacted material with a centrifuge at a speed of 12500r / min, wash it with pure water several times, and then place the solid in an oven and dry it at 60°C for 12h. The obtained powder is a nano metal oxide catalyst, and the components of the nano metal oxide catalyst are: Fe2O3 is 94wt%; CaO is 1.4wt%; SiO2 is 1.2wt%; MgO is 1.0wt%; MnO is 0.5wt%; the remainder is unavoidable impurities.

[0055] The X-ray diffraction pattern of the nano metal oxide catalyst obtained in this comparative example 2 is as follows Figure 4 As shown, the 2θ peaks are located at 24.1°, 33.1°, 35.6°, 40.8°, 49.4°, 54.1°, 57.6°, 62.4° and 64.0°, respectively, belonging to the (012), (104), (110), (113), (024), (116), (018), (214) and (300) crystal planes, respectively, and the synthesis is a nano-metal oxide catalyst with α-Fe2O3 as the main component. The SEM image of the nano-metal oxide synthesized in this comparative example 2 is as follows Figure 5 As shown, from Figure 5 It can be seen that the nanoparticles are in the shape of a round cake with a length of 140nm and a width of 50nm, and the particle size distribution of the catalyst is mainly concentrated between 120 and 160nm.

[0056] In summary, the X-ray diffraction pattern of the nano-metal oxide catalyst obtained in this Example 1 is as follows: Figure 6 As shown, the 2θ peaks are located at 24.1°, 33.1°, 35.6°, 40.8°, 49.4°, 54.1°, 57.6°, 62.4° and 64.0°, respectively, belonging to (012), (104), (110), (113), (024), (116), (018), (214) and (300) crystal planes, respectively, and the synthesis is a nano metal oxide catalyst with α-Fe2O3 as the main component. However, compared with the X-ray diffraction patterns of Comparative Examples 1 and 2, the peak intensity is significantly weakened, and a carbon-related peak appears at 26.0°, proving that oleic acid has effectively modified the nano metal oxide catalyst. The components of the industrial wastewater mentioned above are shown in Table 1 below:

[0057] Table 1

[0058]

[0059]

[0060] Application Example 1

[0061] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst in Comparative Example 1 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 240°C and reacted for 24 hours at 350r / min stirring. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement process, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0062] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0063]

[0064] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0065] The crude oil used in this application example 1 is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 12067mPa·s, and the viscosity reduction rate reaches 70.57%. The SARA results are shown in Table 2. It can be seen that after the reaction, the saturated content and aromatic content of the oil sample are significantly increased, the colloid is significantly reduced, and the asphaltene is also reduced by a certain amount, which is consistent with the result of viscosity reduction and has a good viscosity reduction effect.

[0066] Application Example 2

[0067] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst in Comparative Example 1 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 220°C and reacted for 24 hours at 350r / min stirring. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0068] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0069]

[0070] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0071] The crude oil used in this application example 2 is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 14830mPa·s, and the viscosity reduction rate reaches 63.83%. The SARA results are shown in Table 2. It can be seen that after the reaction, the saturated content and aromatic content of the oil sample are increased, the colloid is reduced, but the asphaltene is not significantly reduced. The temperature reduction is not conducive to the catalytic viscosity reduction effect of the nano metal oxide catalyst.

[0072] Application Example 3

[0073] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst in Comparative Example 1 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 260°C and reacted for 24 hours at 350r / min stirring. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement process, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0074] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0075]

[0076] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0077] The crude oil used in this application example 3 is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 10856mPa·s, and the viscosity reduction rate reaches 73.52%. The SARA results are shown in Table 2. It can be seen that after the reaction, the saturated content and aromatic content of the oil sample are greatly increased, and the colloid and asphaltene are also greatly reduced. The increase in reaction temperature is conducive to the catalytic viscosity reduction effect of the nano metal oxide catalyst.

[0078] Application Example 4

[0079] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst in Comparative Example 2 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 240°C and reacted for 24 hours at 350r / min stirring. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement process, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0080] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0081]

[0082] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0083] The crude oil used in Application Example 4 is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 14227mPa·s, and the viscosity reduction rate reaches 65.3%. The SARA results are shown in Table 2. It can be seen that after the reaction, the saturated content and aromatic content of the oil sample are increased, the colloid is reduced, but the asphaltene is not significantly reduced, indicating that the catalytic viscosity reduction effect of the nano metal oxide catalyst prepared from wastewater is reduced as the size increases.

[0084] Application Example 5

[0085] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst described in Example 1 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 240°C and reacted for 24 hours under stirring at 350r / min. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement process, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0086] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0087]

[0088] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0089] The crude oil used in this application example 5 is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 9717mPa·s, and the viscosity reduction rate reaches 76.3%. The SARA results are shown in Table 2. It can be seen that after the reaction, the saturated content and aromatic content of the oil sample are greatly increased, and the colloid and asphaltene are also greatly reduced. The nano metal oxide modified by oleic acid becomes an oil-soluble catalyst, making it easier to disperse in the oil, thereby improving its heavy oil catalytic viscosity reduction effect.

[0090] Application Example 6

[0091] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and the nano metal oxide catalyst described in Example 2 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The reactor was heated to 240°C and reacted for 24 hours under stirring at 350r / min. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50°C. During the measurement process, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0092] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0093]

[0094] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0095] The crude oil used in this application example is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 10170mPa·s, and the viscosity reduction rate reaches 75.19%. The SARA results are shown in Table 2. The nano metal oxide modified by oleylamine becomes an oil-soluble catalyst, making it easier to disperse in the oil, thereby improving its heavy oil catalytic viscosity reduction effect.

[0096] Application Comparative Example 1

[0097] 80g of heavy oil was placed in a 500mL reactor, water was added at an oil-water ratio of 1:1, and commercial nano-Fe2O3 was added at a mass ratio of heavy oil to catalyst of 1:0.005. The commercial nano-Fe2O3 was from Suzhou Yanxin Materials Industry Co., Ltd. 80nm nano-Fe2O3. The reactor was heated to 240℃ and reacted for 24h under stirring at 350r / min. After the reaction, the oil sample in the reactor was taken out, and the viscosity of the oil sample after the reaction was measured using a viscometer at 50℃. During the measurement, the torque was maintained at 30%-70%, and the changes in the SRAR components of the oil sample were analyzed.

[0098] The viscosity reduction rate (Δη) of the heavy oil viscosity reduction catalyst is calculated by the following formula:

[0099]

[0100] Where η0 is the viscosity before reaction and η is the viscosity after reaction.

[0101] The present invention uses the commercial nano Fe2O3 purchased in comparative example 1, and the SEM image is as follows Figure 8 The sample is a round particle in a stacked state with a size distribution range of 50-200nm.

[0102] The crude oil used in Comparative Example 1 of this application is 41000mPa·s Tuha heavy oil. After the reaction, the viscosity is reduced to 15252mPa·s, and the viscosity reduction rate reaches 62.8%. The SARA results are shown in Table 2. The saturated and aromatic content increases slightly, the colloid content decreases, and the asphaltene content decreases only slightly.

[0103] Table 2

[0104]

[0105]

[0106] Therefore, the viscosity reduction effect of the commercial nano Fe2O3 catalyst in the comparative example 1 is lower than that of the above-mentioned application examples 1 to 6, indicating that the nano metal oxide catalyst mainly composed of Fe2O3 prepared by wastewater is better than the commercial nano Fe2O3 in reducing the viscosity of heavy oil. Compared with application examples 1 to 4, application examples 5 and 6 have a significantly better viscosity reduction effect on heavy oil, and the content of saturated and aromatic components increases most significantly, while the content of colloid and asphaltene is greatly reduced. It can be seen that the nano metal oxide catalyst obtained after modification with oleylamine and oleic acid in application examples 5 and 6 has good oil solubility, which further improves the viscosity reduction rate.

[0107] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.

[0108] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a nano metal oxide catalyst, It is characterized in that The following steps are involved: A. dissolving iron salt in waste water to obtain an iron salt solution, dissolving sodium hydroxide in waste water to obtain a sodium hydroxide solution, and then adding the iron salt solution dropwise to the sodium hydroxide solution to mix well to obtain a mixed solution; B. subjecting the mixed solution of step A to a hydrothermal reaction, centrifuging the reacted material, collecting the precipitate, washing and drying it to obtain a nano-metal oxide catalyst precursor; C. Add the nano metal oxide catalyst precursor in step B to the oil-soluble modifier, centrifuge after the reaction, collect the precipitate, and dry to obtain the nano metal oxide catalyst.

2. The preparation method according to claim 1, It is characterized in that In step A, the iron salt includes at least one of ferric chloride hexahydrate, ferric nitrate nonahydrate and ferric sulfate.

3. The preparation method according to claim 1, It is characterized in that In step A, the mass ratio of the iron salt to the wastewater is (0.01-0.05):

1.

4. The preparation method according to claim 1, It is characterized in that In step A, the molar ratio of sodium hydroxide to iron salt is 3:

1.

5. The preparation method according to claim 1, It is characterized in that In step B, the temperature of the hydrothermal reaction is 140°C to 200°C.

6. The preparation method according to claim 1, It is characterized in that In step B, the hydrothermal reaction time is 6 to 16 hours.

7. The preparation method according to claim 1, It is characterized in that In step C, the oil-soluble modifier includes oleic acid or oleylamine.

8. The preparation method according to claim 1, It is characterized in that In step C, the mass ratio of the oil-soluble modifier to the nano metal oxide catalyst precursor is 1:1 to 3:

1.

9. Use of the nano metal oxide catalyst prepared by the preparation method according to any one of claims 1 to 8 in reducing the viscosity of heavy oil.

Citation Information

Patent Citations

  • Quality-improving and viscosity-reducing catalyst and preparation method thereof

    CN103386323A

  • In-situ composite silicon-based multibasic oxide oxide aerogel material and preparation method thereof

    CN104941538A

  • Nano-fluid thickened oil thermal recovery assistant and preparation method thereof

    CN105542743A

  • Preparation method and application of thick oil viscosity reducer

    CN114058357A

  • Catalyst for downhole catalytic reforming of viscous crude

    CN1843622A

Cited By

  • Enhanced composite nano material based on petal-shaped MoS2, preparation method and application

    CN121714699A