Catalyst for degrading COD (Chemical Oxygen Demand) in wastewater and preparation method of catalyst

By preparing niobium pentoxide and carbon-doped hafnium disulfide composite materials, the existing photocatalytic oxidation catalysts have been solved, and efficient degradation of COD in wastewater and long-term stable use is achieved.

CN118904357AActive Publication Date: 2024-11-08CANGZHOU JULONG CHEM IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410944278.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

When the existing photocatalytic oxidation catalysts treat difficult biodegradation organic matter in wastewater, there are problems such as poor pollution resistance, easy deactivation and short service life, which are difficult to meet the requirements of industrial applications.

Method used

Using niobium pentoxide and carbon-doped hafnium disulfide composite material as catalyst, it is prepared by hydrothermal reaction and high-temperature sintering process to form a carbon-doped hafnium disulfide catalyst with high specific surface area and strong activity, for degradation of wastewater. COD.

Benefits of technology

This catalyst exhibits good catalytic degradation efficiency in treating wastewater, is not easy to be deactivated, has a long service life and good reusability, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945153790000071
    Figure BDA0004945153790000071
Patent Text Reader

Abstract

The invention relates to a catalyst for degrading COD (Chemical Oxygen Demand) in wastewater and a preparation method of the catalyst. The preparation method comprises the following steps: 1, preparing niobium pentoxide; 2, preparing a pre-reaction liquid: weighing octadecyl trimethyl ammonium chloride, thioacetamide and distilled water, mixing, uniformly stirring, adding niobium pentoxide powder, and uniformly stirring to obtain a mixed liquid A; weighing hafnium oxychloride octahydrate, mixing the hafnium oxychloride octahydrate with distilled water, and fully stirring to obtain a mixed solution B; mixing the mixed solution B with the mixed solution A to obtain a mixed solution C; 3, hydrothermal reaction: pouring the mixed solution C into a reaction kettle, and carrying out heating reaction to obtain a product D; and 4, sintering at high temperature to obtain niobium pentoxide / carbon doped hafnium disulfide. The photocatalyst disclosed by the invention is a composite product of carbon-doped hafnium disulfide and niobium pentoxide, not only has relatively good catalytic degradation efficiency on organic pollutants in wastewater, but also is not easy to inactivate, has very good reusability and is relatively long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of wastewater degradation, and in particular to a catalyst for degrading COD in wastewater and a preparation method thereof. Background Art

[0002] After the biochemical treatment of industrial wastewater and municipal sewage, the effluent still contains a certain concentration of organic matter, which is generally difficult to biodegrade and constitutes the main chemical oxygen demand (COD) of the effluent from the biochemical treatment. With the continuous improvement of the discharge standards for industrial wastewater and municipal sewage, the effluent COD of the biochemical treatment system is often difficult to meet the discharge standards, and the demand for reclaimed water reuse is also expanding. Objectively, it is also necessary to add deep treatment units after the biochemical treatment of industrial wastewater and municipal sewage. The deep treatment technologies for wastewater and sewage mainly include three types of technologies: adsorption, membrane separation and advanced oxidation.

[0003] Adsorption technology is a relatively mature deep treatment technology that can economically and effectively remove odors, decolorize, and separate heavy metals and organic pollutants. However, the cost of adsorbents (such as granular activated carbon, activated carbon fiber, and resin) is high, and adsorbent regeneration is difficult. The solid waste that is inevitably produced is a difficult secondary pollution, and pollutants are not eliminated in essence. Membrane separation technology is divided into microfiltration, ultrafiltration, nanofiltration, and reverse osmosis technology according to the pore size of the filter membrane. Its characteristics are a wide range of separation objects and good effluent quality, but the investment and operating costs are high, the life of the membrane is not long, and it is inevitable that "concentrated water" with high organic matter concentration and salt concentration will be produced. The treatment and disposal of "concentrated water" is a difficult problem. This technology essentially concentrates pollutants into "concentrated water". The most commonly used advanced oxidation technology is photocatalytic oxidation, which not only has a fast reaction speed, but also usually does not produce secondary pollution. It is especially suitable for treating organic matter that is difficult to biodegrade.

[0004] Currently, the most commonly used catalyst for photocatalytic oxidation is nanometal oxide. Although nanometal oxide photocatalytic materials can catalytically degrade organic pollutants in wastewater to a certain extent, they still have problems such as being not resistant to pollution, easy to deactivate and having a short service life, making it difficult to meet industrial application requirements. Summary of the invention

[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a catalyst for degrading COD in wastewater and a preparation method thereof.

[0006] The purpose of the present invention is achieved by adopting the following technical solutions:

[0007] In a first aspect, the present invention discloses a method for preparing a catalyst for degrading COD in wastewater, comprising the following steps:

[0008] The first step is to prepare niobium pentoxide:

[0009] Weigh niobium pentoxide hydrogen, grind it, sieve it, collect it into a crucible, and then place it in a muffle furnace for heating treatment. After cooling in the furnace, niobium pentoxide powder is obtained;

[0010] The second step is to prepare the pre-reaction solution:

[0011] Weigh octadecyltrimethylammonium chloride, thioacetamide and distilled water, mix them, stir them evenly, add niobium pentoxide powder, stir them again until they are evenly mixed, and obtain a mixed solution A; weigh hafnium oxychloride octahydrate and distilled water, mix them, stir them thoroughly, and obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A, and stir them evenly after the dropwise addition is completed, and obtain a mixed solution C;

[0012] The third step, hydrothermal reaction:

[0013] Pour the mixed solution C into a reactor and heat it for reaction. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it to obtain product D.

[0014] Step 4: High temperature sintering:

[0015] The product D is placed in a muffle furnace and subjected to a temperature-raising treatment under the protection of a rare gas. After the reaction is completed, the product is ground and sieved to obtain niobium pentoxide / carbon-doped hafnium disulfide.

[0016] Preferably, in the first step, the purity of niobium pentoxide hydrogen is higher than 99.9%, and after grinding, it passes through a 250-300 mesh sieve.

[0017] Preferably, in the first step, the conditions in the muffle furnace are: under air conditions, firstly heating to 350-550°C, keeping the temperature for 1-2 hours, then heating to 600-800°C, keeping the temperature for 2-4 hours.

[0018] Preferably, in the mixed solution A of the second step, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1 g: (0.1-0.3) g: (0.8-1.6) g: (50-100) mL.

[0019] Preferably, in the mixed solution B of the second step, the mass volume ratio of hafnium oxychloride octahydrate to distilled water is (0.4-0.8) g: (50-100) mL.

[0020] Preferably, in the mixed solution C of the second step, the dropping speed is 40-80 drops / minute, and stirring is continued for 1-2 hours after the dropping is completed.

[0021] Preferably, in the third step, the temperature in the reactor is set to 180-260° C., and the reaction time is set to 15-30 h.

[0022] Preferably, in the fourth step, the sintering temperature is 750-850° C., and the sintering time is 1.5-3.5 hours.

[0023] Preferably, in the fourth step, the rare gas is one of helium, neon, argon, krypton and xenon.

[0024] Preferably, in the fourth step, the powder is ground and then sieved through a 100-150 mesh screen.

[0025] In a second aspect, the present invention discloses a catalyst for degrading COD in wastewater, which is prepared by the above method.

[0026] In a third aspect, the present invention discloses the application of a catalyst for degrading COD in wastewater in organic wastewater.

[0027] The beneficial effects of the present invention are:

[0028] 1. The present invention prepares a catalyst capable of degrading COD in wastewater. The catalyst is a photocatalyst material, and the material body is a composite product of carbon-doped hafnium disulfide and niobium pentoxide. It not only has good catalytic degradation efficiency for ammonia nitrogen and COD in wastewater, but also is not easy to deactivate, has very good reusability, and has a long service life.

[0029] 2. The catalyst prepared by the present invention uses niobium pentoxide as a matrix and is composited with carbon-doped hafnium disulfide in an in-situ generated manner to finally prepare a composite product. Compared with traditional metal oxides, it has a higher specific surface area, stronger activity, convenient post-processing, and can be put into use for a longer period of time.

[0030] 3. In the present invention, carbon-doped hafnium disulfide is prepared by adding octadecyltrimethylammonium chloride during the preparation of hafnium disulfide. On the one hand, it acts as a surfactant to enhance the dispersibility, and on the other hand, it can introduce a long-chain carbon polymer, thereby carbonizing to form a carbon intercalation layer during the subsequent sintering process, thereby obtaining carbon-doped hafnium disulfide. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0032] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0033] The present invention will be further described below in conjunction with the following examples.

[0034] Example 1

[0035] A method for preparing a catalyst for degrading COD in wastewater comprises the following steps:

[0036] The first step is to prepare niobium pentoxide:

[0037] Weigh niobium pentoxide H5Nb3O 10 (with a purity higher than 99.9%), after grinding, pass through a 300-mesh sieve, collect into a crucible, and then place in a muffle furnace, under air conditions, first heat to 350-550°C, keep warm for 1-2 hours, then heat to 600-800°C, keep warm for 2-4 hours, and cool with the furnace to obtain niobium pentoxide Nb2O5 powder;

[0038] The second step is to prepare the pre-reaction solution:

[0039] Weigh octadecyltrimethylammonium chloride STAC, thioacetamide TAA and distilled water, mix them, stir them evenly, add niobium pentoxide Nb2O5 powder, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1g:0.2g:1.2g:80mL, stir them again until they are evenly mixed to obtain a mixed solution A; weigh hafnium oxychloride octahydrate Cl2HfO·8H2O and mix them with distilled water, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.6g:80mL, stir them thoroughly to obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A at a dropping speed of 60 drops / minute, and continue stirring for 1.5h after the dropping is completed to obtain a mixed solution C;

[0040] The third step, hydrothermal reaction:

[0041] Pour the mixed solution C into the reactor and keep it at 220°C for 24 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 100°C to obtain product D.

[0042] Step 4: High temperature sintering:

[0043] The product D was placed in a muffle furnace, heated to 800°C under the protection of a rare gas, and kept warm for 2.5 hours. After the reaction was completed, it was ground into powder and passed through a 100-mesh sieve to obtain niobium pentoxide / carbon-doped hafnium disulfide Nb2O5 / C-HfS2.

[0044] Example 2

[0045] A method for preparing a catalyst for degrading COD in wastewater comprises the following steps:

[0046] The first step is to prepare niobium pentoxide:

[0047] Weigh niobium pentoxide (with a purity higher than 99.9%), grind it, pass it through a 250-mesh sieve, collect it in a crucible, and then place it in a muffle furnace. Heat it to 350° C. in air and keep it warm for 4 hours. After cooling it in the furnace, niobium pentoxide powder is obtained.

[0048] The second step is to prepare the pre-reaction solution:

[0049] Weigh octadecyltrimethylammonium chloride, thioacetamide and distilled water, mix them, stir them evenly, add niobium pentoxide powder, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1g:0.1g:0.8g:50mL, stir them again until they are evenly mixed to obtain a mixed solution A; weigh hafnium oxychloride octahydrate and distilled water, mix them, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.4g:50mL, stir them thoroughly to obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A at a dropping speed of 40 drops / minute, and continue stirring for 1h after the dropping is completed to obtain a mixed solution C;

[0050] The third step, hydrothermal reaction:

[0051] Pour the mixed solution C into the reactor and keep the temperature at 180°C for 30 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 80°C to obtain product D.

[0052] Step 4: High temperature sintering:

[0053] The product D was placed in a muffle furnace, and under the protection of a rare gas, the temperature was raised to 750°C and kept warm for 3.5 hours. After the reaction was completed, it was ground into powder and passed through a 100-mesh sieve to obtain niobium pentoxide / carbon-doped hafnium disulfide.

[0054] Example 3

[0055] A method for preparing a catalyst for degrading COD in wastewater comprises the following steps:

[0056] The first step is to prepare niobium pentoxide:

[0057] Weigh niobium pentoxide (with a purity higher than 99.9%), grind it, pass it through a 300-mesh sieve, collect it in a crucible, and then place it in a muffle furnace. Heat it to 500° C. in air and keep it warm for 3 hours. After cooling it in the furnace, niobium pentoxide powder is obtained.

[0058] The second step is to prepare the pre-reaction solution:

[0059] Weigh octadecyltrimethylammonium chloride, thioacetamide and distilled water, mix them, stir them evenly, add niobium pentoxide powder, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1g:0.2g:1g:60mL, stir them again until they are evenly mixed to obtain a mixed solution A; weigh hafnium oxychloride octahydrate and distilled water, mix them, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.5g:60mL, stir them thoroughly to obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A at a dropping speed of 70 drops / minute, and continue stirring for 1-2h after the dropping is completed to obtain a mixed solution C;

[0060] The third step, hydrothermal reaction:

[0061] Pour the mixed solution C into the reactor and keep it at 200°C for 28 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 120°C to obtain product D.

[0062] Step 4: High temperature sintering:

[0063] The product D was placed in a muffle furnace, and under the protection of a rare gas, the temperature was raised to 800°C and kept warm for 2 hours. After the reaction was completed, the product was ground into powder and passed through a 150-mesh sieve to obtain niobium pentoxide / carbon-doped hafnium disulfide.

[0064] Example 4

[0065] A method for preparing a catalyst for degrading COD in wastewater comprises the following steps:

[0066] The first step is to prepare niobium pentoxide:

[0067] Weigh niobium pentoxide (with a purity higher than 99.9%), grind it, pass it through a 300-mesh sieve, collect it in a crucible, and then place it in a muffle furnace. Heat it to 550° C. in air and keep it warm for 2 hours. After cooling it in the furnace, niobium pentoxide powder is obtained.

[0068] The second step is to prepare the pre-reaction solution:

[0069] Weigh octadecyltrimethylammonium chloride, thioacetamide and distilled water, mix them, stir them evenly, add niobium pentoxide powder, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1g:0.3g:1.6g:100mL, stir them again until they are evenly mixed to obtain a mixed solution A; weigh hafnium oxychloride octahydrate and distilled water, mix them, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.8g:100mL, stir them thoroughly to obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A at a dropping speed of 80 drops / minute, and continue stirring for 2h after the dropping is completed to obtain a mixed solution C;

[0070] The third step, hydrothermal reaction:

[0071] Pour the mixed solution C into the reactor and keep the temperature at 260°C for 30 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 120°C to obtain product D.

[0072] Step 4: High temperature sintering:

[0073] The product D was placed in a muffle furnace, and under the protection of a rare gas, the temperature was raised to 850°C and kept warm for 1.5 hours. After the reaction was completed, it was ground into powder and passed through a 150-mesh sieve to obtain niobium pentoxide / carbon-doped hafnium disulfide.

[0074] Comparative Example 1

[0075] A catalyst for degrading COD in wastewater is niobium pentoxide Nb2O5 powder, and the specific preparation process is the same as that of Example 1.

[0076] Comparative Example 2

[0077] A catalyst for degrading COD in wastewater is carbon-doped hafnium disulfide C-HfS2, and the specific preparation process includes:

[0078] The first step is to prepare the pre-reaction solution:

[0079] Weigh octadecyltrimethylammonium chloride STAC, thioacetamide TAA and distilled water, mix them, stir them evenly, the mass volume ratio of octadecyltrimethylammonium chloride, thioacetamide and distilled water is 0.2g:1.2g:80mL, stir them again until they are even, and obtain a mixed solution A; weigh hafnium oxychloride octahydrate Cl2HfO·8H2O and distilled water, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.6g:80mL, and stir them thoroughly to obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A at a dropping speed of 60 drops / minute, and continue stirring for 1.5h after the dropping is completed to obtain a mixed solution C;

[0080] The second step is hydrothermal reaction:

[0081] Pour the mixed solution C into the reactor and keep it at 220°C for 24 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 100°C to obtain product D.

[0082] The third step, high temperature sintering:

[0083] The product D was placed in a muffle furnace, heated to 800°C under the protection of a rare gas, and kept warm for 2.5 hours. After the reaction was completed, it was ground into powder and passed through a 100-mesh sieve to obtain carbon-doped hafnium disulfide C-HfS2.

[0084] Comparative Example 3

[0085] A catalyst for degrading COD in wastewater is niobium pentoxide / hafnium disulfide Nb2O5 / HfS2. The preparation process is different from that of Example 1 only in that octadecyltrimethylammonium chloride is not added. The specific preparation process includes:

[0086] The first step is to prepare niobium pentoxide, which is the same as Example 1.

[0087] The second step is to prepare the pre-reaction solution:

[0088] Weigh thioacetamide TAA and distilled water, mix them, stir them evenly, add niobium pentoxide Nb2O5 powder, the mass volume ratio of niobium pentoxide powder, thioacetamide and distilled water is 1g:1.2g:80mL, stir them again until they are evenly mixed, and obtain a mixed solution A; weigh hafnium oxychloride octahydrate Cl2HfO·8H2O and distilled water, the mass volume ratio of hafnium oxychloride octahydrate and distilled water is 0.6g:80mL, stir them thoroughly, and obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A, the dropping speed is 60 drops / minute, and continue stirring for 1.5h after the dropping is completed, and obtain a mixed solution C;

[0089] The third step, hydrothermal reaction:

[0090] Pour the mixed solution C into the reactor and keep it at 220°C for 24 hours. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it at 100°C to obtain product D.

[0091] Step 4: High temperature sintering:

[0092] The product D was placed in a muffle furnace, and under the protection of a rare gas, the temperature was raised to 800°C and kept warm for 2.5 hours. After the reaction was completed, it was ground into powder and passed through a 100-mesh sieve to obtain niobium pentoxide / hafnium disulfide Nb2O5 / HfS2.

[0093] In order to more clearly illustrate the present invention, corresponding tests were performed on the catalysts of Example 1 of the present invention and Comparative Examples 1-3.

[0094] The detection process is as follows:

[0095] (1) Chemical industrial wastewater was used as the experimental wastewater source. The initial concentration of ammonia nitrogen in the detected wastewater was 227 mg / L, and the initial concentration of COD was 623 mg / L.

[0096] (2) The experimental wastewater source was divided into four equal parts, and the catalysts prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were added respectively, and then stirred evenly. The mass concentration of the catalyst was 80 mg / L, and then each wastewater source was marked respectively.

[0097] (3) Expose each wastewater source under ultraviolet light at an irradiation dose of 120 mW / cm 2 The distance between the light source and the water source was 30 cm, the temperature was set to 35 °C, and the degradation treatment was carried out under stirring conditions.

[0098] (4) Start the degradation treatment and measure the ammonia nitrogen concentration and COD concentration in the wastewater source at 30 minutes and 60 minutes of treatment, respectively, and record them as the ammonia nitrogen degradation concentration and COD degradation concentration, and then calculate the degradation percentage according to the formula:

[0099] Ammonia nitrogen degradation rate (%) = (initial ammonia nitrogen concentration - ammonia nitrogen degradation concentration) / initial ammonia nitrogen concentration × 100%;

[0100] COD degradation rate (%) = (COD initial concentration - COD degradation concentration) / COD initial concentration × 100%.

[0101] The test results are shown in Table 1:

[0102] Table 1 Efficiency of catalysts in degrading wastewater

[0103]

[0104] (5) After the wastewater treatment, the catalyst was filtered and collected, and then soaked in acetone and ultrasonicated for 0.5 h, and then dried and put into use again. After being reused 10 times in the manner of step (2), the ammonia nitrogen and COD degradation efficiency of the wastewater were tested again after 60 min. The test results are shown in Table 2:

[0105] Table 2 Degradation efficiency of the catalyst after repeated use 10 times

[0106] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Ammonia nitrogen degradation rate 98.1% 92.0% 92.8% 95.8% COD degradation rate 92.7% 84.9% 87.1% 89.2%

[0107] Result analysis:

[0108] It can be seen from Table 1 that the degradation rate of ammonia nitrogen by the catalyst prepared in Example 1 of the present invention reached 93.8% at 30 minutes and 98.9% at 60 minutes; the degradation rate of COD reached 87.3% at 30 minutes and 93.5% at 60 minutes. It shows that the catalyst prepared in Example 1 of the present invention has very good photocatalytic efficiency and is better than the performance of other comparative examples. And it can be seen from Table 2 that the catalyst prepared in Example 1 of the present invention can still maintain a high ammonia nitrogen degradation rate and COD degradation rate after ten times of repeated use, which shows that it is highly reusable, not easy to deactivate, and has a long service life.

[0109] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0110] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a catalyst for degrading COD in wastewater, characterized in that: The following steps are involved: The first step is to prepare niobium pentoxide: Weigh niobium pentoxide hydrogen, grind it, sieve it, collect it into a crucible, and then place it in a muffle furnace for heating treatment. After cooling in the furnace, niobium pentoxide powder is obtained; The second step is to prepare the pre-reaction solution: Weigh octadecyltrimethylammonium chloride, thioacetamide and distilled water, mix them, stir them evenly, add niobium pentoxide powder, stir them again until they are evenly mixed, and obtain a mixed solution A; weigh hafnium oxychloride octahydrate and distilled water, mix them, stir them thoroughly, and obtain a mixed solution B; gradually drop the mixed solution B into the continuously stirred mixed solution A, and stir them evenly after the dropwise addition is completed, and obtain a mixed solution C; The third step, hydrothermal reaction: Pour the mixed solution C into a reactor and heat it for reaction. After the reaction is completed, filter the reaction solution in the reactor, wash it with water three times, and dry it to obtain product D. Step 4: High temperature sintering: The product D is placed in a muffle furnace and subjected to a temperature-raising treatment under the protection of a rare gas. After the reaction is completed, the product is ground and sieved to obtain niobium pentoxide / carbon-doped hafnium disulfide.

2. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the first step, the purity of niobium pentoxide is higher than 99.9%, and after grinding, it passes through a 250-300 mesh sieve.

3. The method for preparing a catalyst for degrading COD in waste water according to claim 1, characterized in that: In the first step, the conditions in the muffle furnace are: under air conditions, firstly heating to 350-550° C., keeping the temperature for 1-2 hours, then heating to 600-800° C., keeping the temperature for 2-4 hours.

4. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the mixed solution A of the second step, the mass volume ratio of niobium pentoxide powder, octadecyltrimethylammonium chloride, thioacetamide and distilled water is 1g:(0.1-0.3)g:(0.8-1.6)g:(50-100)mL.

5. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the mixed solution B of the second step, the mass volume ratio of hafnium oxychloride octahydrate to distilled water is (0.4-0.8) g: (50-100) mL.

6. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the mixed solution C of the second step, the dropping speed is 40-80 drops / minute, and stirring is continued for 1-2 hours after the dropping is completed.

7. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the third step, the temperature in the reactor is set to 180-260° C., and the reaction time is set to 15-30 h.

8. The method for preparing a catalyst for degrading COD in wastewater according to claim 1, characterized in that: In the fourth step, the sintering temperature is 750-850° C., and the sintering time is 1.5-3.5 hours.

9. A catalyst for degrading COD in wastewater according to claim 1, characterized in that: It is prepared by the above method.

10. Use of the catalyst for degrading COD in wastewater according to claim 1 in organic wastewater.

Citation Information

Patent Citations

  • Organic wastewater COD degradation catalyst and preparation method thereof

    CN112237915A

  • Semiconductor memory device

    CN115696911A

  • Method of producing inorganic fullerene-type nanostructures of metal disulphides, nanostructures produced thereby and use thereof

    WO2009152999A2