Preparation method of super-hydrophobic metal organic framework zinc electrode protective coating

By modifying fluorophorescent silane on the surface of metal organic frame materials and preparing superhydrophobic F-MOF coating, the corrosion and zinc dendrites of zinc are solved, and the cycle life of zinc anode, the corrosion resistance and electrochemical properties of the battery are significantly improved. .

CN118904684APending Publication Date: 2024-11-08NORTH CHINA ELECTRIC POWER UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111403.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08

Smart Images

  • Figure CN118904684A_ABST
    Figure CN118904684A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-hydrophobic metal organic framework zinc electrode protective coating. The preparation method comprises the following steps: firstly, sequentially adding an N, N-dimethylformamide solution, ZrCl4 and H2BDC into a reaction container, dropwise adding concentrated hydrochloric acid, stirring, transferring the mixture into a stainless steel high-pressure kettle lined with polytetrafluoroethylene, heating to 120 DEG C, reacting for 24 hours, and centrifugally collecting metal organic framework powder; then mixing the nano MOF particles with ethanol and a fluorosilane modifier, performing ultrasonic treatment and stirring, and drying to obtain fluorosilane modified nano MOF particles; and finally, mixing the F-MOF nanoparticles with an organic solvent, and spraying the mixture on a zinc foil substrate by using a spray gun to prepare the zinc electrode with the super-hydrophobic metal organic framework coating. The prepared F-MOF nano-particles accelerate zinc ion transmission by promoting desolvation of [Zn (H2O) 6] < 2 + > hydrate, so that hydrogen evolution reaction and zinc dendrite formation are inhibited, and the cycling stability of a zinc anode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating. Background Art

[0002] Aqueous zinc batteries (AZBs) show great application potential in the field of large-scale energy storage due to their low cost, high safety and sustainability. However, the zinc anode is prone to corrosion and zinc dendrite formation during the cycle process, which not only affects the cycle life of the battery, but may also lead to short circuit and failure of the battery. Therefore, finding effective methods to stabilize the zinc anode interface and inhibit the growth of zinc dendrites has become the focus of current research. At present, the use of interface modification methods, such as coating a protective layer, is an effective means to improve the stability of the zinc anode. Metal-organic framework (MOF) materials have become an ideal coating material due to their unique structural and functional properties, but their water resistance is limited and it is difficult to completely inhibit water erosion.

[0003] In order to overcome this problem, the present invention proposes a method for preparing a super-hydrophobic F-MOF coating by modifying the MOF surface with fluorinated silane. The coating can not only provide uniform Zn 2+ The transmission channel also has excellent hydrophobic properties, which effectively inhibits the hydrogen evolution reaction and the formation of zinc dendrites, thereby significantly improving the cycle life and electrochemical performance of the zinc anode. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating.

[0005] A method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating comprises the following steps:

[0006] S1. Prepare substrate materials, and polish and clean the substrate surface. The treated surface is recorded as A for standby use.

[0007] S2. In a reaction container, add the following ingredients in the following order: N,N-dimethylformamide (DMF) solution, ZrCl4 and H2BDC, and stir thoroughly to obtain a solution, which is designated as B and is set aside;

[0008] S3. Slowly add concentrated hydrochloric acid solution to solution B while stirring at an appropriate speed until all components are evenly dissolved to form a transparent solution. The resulting solution is recorded as C for later use.

[0009] S4, the fully stirred solution C was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, heated to 120°C for reaction for 24 hours, cooled naturally to room temperature, and the metal organic framework powder (MOF) was collected by centrifugation and recorded as D for later use;

[0010] S5, adding ethanol and fluorosilane modifier to the nanoparticles D, stirring until the nanoparticles are evenly dispersed, repeating ultrasonic treatment and stirring for multiple times, and then drying to obtain fluorosilane-modified nano-MOF particles (F-MOF), which are recorded as E and set aside;

[0011] S6, mixing the fluorosilane-modified nano-MOF particles with an organic solvent, stirring them sufficiently to disperse them, and obtaining a dispersion, which is referred to as solution F, for later use;

[0012] S7. Use a spray gun to spray solution F onto a zinc foil substrate to obtain a zinc electrode with a superhydrophobic metal-organic framework coating.

[0013] Furthermore, in step S1, the substrate material is zinc foil, and the thickness is between 0.2 mm and 1 mm. The polishing and cleaning treatment includes: polishing the surface by grinding or belt grinding until the roughness Ra value is less than 0.64 μm, and then ultrasonically cleaning in anhydrous ethanol and deionized water in turn, each cleaning for 20-30 minutes, and drying naturally for standby use.

[0014] Furthermore, in step S3, during the process of adding concentrated hydrochloric acid, the pH value is adjusted to 3-4.

[0015] Furthermore, in the steps S2-S6, sufficient stirring is magnetic stirring at a speed of 1000 rpm for 30-50 min; repeated ultrasonic treatment and stirring are ultrasonic treatment for 10-20 min, followed by magnetic stirring at a speed of 1000 rpm for 10-20 min, and repeated 3-5 times.

[0016] Furthermore, in steps S4 and S5, the size of the prepared MOF nanoparticles and F-MOF nanoparticles is about 20 μm.

[0017] Furthermore, in steps S4 and S5, the prepared MOF nanoparticles and F-MOF nanoparticles can promote uniform deposition of zinc ions due to their regular channels.

[0018] Furthermore, in step S5, the prepared F-MOF nanoparticles can promote [Zn(H2O)6] 2+ Hydrate desolvation accelerates zinc ion transfer.

[0019] Beneficial effects of the present invention: The present invention provides a super-hydrophobic metal organic framework zinc electrode protective coating and a preparation method thereof, and the beneficial effects include:

[0020] 1. The present invention uses a hydrophobic F-MOF coating to effectively inhibit hydrogen evolution reaction and zinc corrosion, extend the service life of the zinc anode, and improve the corrosion resistance of the battery.

[0021] 2. The hydrophobic F-MOF coating of the present invention has regular ion transmission channels, promotes uniform deposition of zinc ions, prevents the formation of dendrites, and improves the safety of the battery.

[0022] 3. The present invention discloses a super-hydrophobic metal organic framework zinc electrode protective coating and a preparation method thereof, wherein the super-hydrophobic coating F-MOF promotes [Zn(H2O)6] 2+ Hydrate desolvation accelerates zinc ion transfer and significantly improves the electrochemical performance of the battery, enabling it to maintain good capacity and cycle life at high current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of superhydrophobic metal-organic framework.

[0024] Figure 2 Scanning electron microscope image of the surface microstructure of the super-hydrophobic MOF coating prepared in Example 1.

[0025] Figure 3 Example 1 Corrosion resistance test results of super hydrophobic MOF coating prepared.

[0026] Figure 4 Example 1: Cyclic stability test results of symmetric battery of zinc electrode prepared with superhydrophobic MOF coating. DETAILED DESCRIPTION

[0027] In order to have a more thorough and comprehensive understanding of the disclosure of the present invention, the present invention is further described below in conjunction with the embodiments and drawings. It should be noted that the present invention can be implemented in many different forms, and the embodiments listed herein cannot be understood as limiting the scope of this patent. Obviously, a person of ordinary skill in the art can obtain other embodiments according to the present invention without paying creative work.

[0028] Embodiment 1:

[0029] A method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating is specifically carried out according to the following steps:

[0030] S1. Select a zinc foil with a thickness of 0.5 mm, and use a grinding process to finish the surface until the roughness Ra value is less than 0.64 μm. Then, ultrasonically clean it in anhydrous ethanol and deionized water in turn, each time for 20 minutes. The surface treated in this way is recorded as A, and it is naturally dried for use;

[0031] S2. In a 200 ml reaction container, add the following ingredients in the following order: 80 ml N,N-dimethylformamide (DMF) solution, 3.094 g ZrCl4 and 4.412 g H2BDC, and stir magnetically at 1000 rpm for 30-50 min at room temperature to obtain a clear solution, which is recorded as B and set aside;

[0032] S3. At room temperature, under magnetic stirring at a speed of 1000 rpm, concentrated hydrochloric acid solution was gradually added to solution B, and the pH value of the solution was monitored using a pH meter until the pH value reached 7, all components were uniformly dissolved and a transparent solution was formed, and the obtained solution was recorded as C for standby use;

[0033] S4, transfer the fully stirred solution C to a stainless steel autoclave lined with polytetrafluoroethylene, heat to 120°C for 24h, cool naturally to room temperature, centrifuge and repeatedly wash with DMF solution, collect the white metal organic framework (MOF) powder, record it as D, and set aside;

[0034] S5, adding 0.2 g of nanoparticle D and 0.1 g of fluorosilane modifier to 10 ml of anhydrous ethanol, ultrasonically treating for 10-20 min, and then magnetically stirring at a speed of 1000 rpm for 10-20 min, repeating 3-5 times and drying to obtain fluorosilane-modified nano-MOF particles (F-MOF), recorded as E, for later use;

[0035] S6, mixing the fluorosilane-modified nano-MOF particles and an organic solvent at a ratio of 1:10, and dispersing them by magnetic stirring at a speed of 1000 rpm for 30-50 min at room temperature to obtain a dispersion liquid, which is recorded as dispersion liquid F and set aside;

[0036] S7, using a spray gun to spray the uniform dispersion F onto the zinc foil at a pressure of 0.5 MPa, drying at room temperature for 8 hours, and then drying in a vacuum drying oven at 80° C. for 30 minutes to obtain a super hydrophobic metal organic framework zinc electrode protective coating, recorded as F-MOF@zinc electrode ( Figure 1-2 ).

[0037] Experimental example:

[0038] Corrosion resistance test of super-hydrophobic coating: According to the steps of preparing the base coating in Example 1, a zinc electrode (F-MOF@zinc electrode) with a size of about 5 cm*5 cm*0.5 mm and having a super-hydrophobic metal organic framework coating was prepared. The scanning rate was 1 mV s -1, a three-electrode structure was adopted (Pt foil as symmetric electrode, Ag / AgCl as reference electrode, and zinc electrode with superhydrophobic metal-organic framework coating as working electrode), and the Tafel plot was linearly fitted to obtain the corrosion current density. Figure 3 Tafel plots of the corrosion behavior of bare Zn and F-MOF@Zn electrodes in 2 M ZnSO4 electrolyte were recorded.

[0039] In this section, the corrosion resistance of the zinc electrode of the superhydrophobic metal organic framework zinc electrode protective coating described in the present invention is analyzed. The corrosion current density observed on the F-MOF@zinc electrode is 0.62 mA cm -2 , which is significantly lower than the corrosion current density of 3.62 mA cm on bare zinc. -2 The presence of F-MOF not only significantly reduced the corrosion current density, but also shifted the corrosion potential from -1.092 V on bare zinc to -0.981 V on F-MOF@Zn electrode (vs. Ag / AgCl). This indicates that the prepared coating inhibits hydrogen evolution reaction and corrosion reaction and has excellent corrosion resistance.

[0040] Symmetrical battery cycling stability test of zinc electrode with superhydrophobic coating: 2M ZnSO4 was used as electrolyte, glass fiber was used as separator, and two identical zinc foils with superhydrophobic metal organic framework coating (F-MOF@zinc electrode) were used as positive and negative electrodes to assemble into a symmetrical battery. -2 (Area capacity: 0.5mAh cm -2 ) was used to test its cycling stability at a current density of 1.5 200 Hz. The cycle life of the symmetrical cell with F-MOF@Zn electrode exceeded 2000 h, significantly exceeding the cycle life of the bare zinc symmetrical cell of 225 h ( Figure 4 ). In addition, the F-MOF coating reduced the polarization voltage of the battery and increased the stability of the F-MOF@Zn electrode symmetric battery (49 mV). This difference is mainly due to the fact that the F-MOF coating promotes the Zn 2+ The desolvation process accelerates the transport of ions.

[0041] The detailed description of the above embodiments and experimental examples is for better understanding and use of the present invention. It is particularly pointed out here that for ordinary technicians in the field, without departing from the design spirit of the present invention, making several variations and modifications to the present invention should fall within the protection scope of the present invention. The protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating, characterized in that: The following steps are involved: S1. Prepare substrate materials, and polish and clean the substrate surface. The treated surface is recorded as A for standby use. S2. In a reaction container, add the following ingredients in the following order: N,N-dimethylformamide solution, ZrCl4 and H2BDC, and stir thoroughly to obtain a solution, which is recorded as B and set aside; S3, adding concentrated hydrochloric acid solution dropwise to solution B, stirring thoroughly, until all components are uniformly dissolved to form a transparent solution, and the resulting solution is recorded as C for later use; S4, transfer solution C to a stainless steel autoclave lined with polytetrafluoroethylene, heat to 120°C for 24 hours, cool naturally to room temperature, and collect the metal organic framework powder by centrifugation, record it as D, and set aside; S5, adding ethanol and fluorosilane modifier to powder D, stirring until dispersed evenly, repeating ultrasonic treatment and stirring for multiple times and then drying to obtain fluorosilane-modified nano-MOF particles, recorded as E, for later use; S6, mixing the particles E with an organic solvent, stirring them sufficiently to disperse them, and obtaining a dispersion, which is referred to as solution F and is set aside; S7. Use a spray gun to spray solution F onto a zinc foil substrate to obtain a zinc electrode with a superhydrophobic metal-organic framework coating.

2. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In the step S1, the substrate material is zinc foil with a thickness between 0.2 mm and 1 mm.

3. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In step S1, the surface grinding and cleaning treatment includes: flattening the surface by grinding or belt grinding until the roughness Ra value is less than 0.64 μm, and then ultrasonically cleaning in anhydrous ethanol and deionized water in turn, each cleaning time is 20-30 minutes, and then naturally drying for use.

4. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In step S3, during the process of adding concentrated hydrochloric acid, the pH value is adjusted to 3-4.

5. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In the steps S2-S6, sufficient stirring is magnetic stirring at a speed of 1000 rpm for 30-50 min; repeated ultrasonic treatment and stirring are ultrasonic treatment for 10-20 min, followed by magnetic stirring at a speed of 1000 rpm for 10-20 min, and repeated 3-5 times.

6. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In the steps S4 and S5, the prepared metal organic framework powder and fluorosilane-modified nano-MOF particles have a size of 15-25 μm.

7. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In the steps S4 and S5, the prepared metal organic framework powder and fluorosilane-modified nano-MOF particles promote uniform deposition of zinc ions.

8. The method for preparing a super-hydrophobic metal organic framework zinc electrode protective coating according to claim 1, characterized in that: In step S5, the prepared fluorosilane-modified nano-MOF particles promote the [Zn(H2O)6] 2+ Hydrate desolvation accelerates zinc ion transfer.