Rectangular flat steel hole pattern design and rolling process
By rationally designing the roll pass of rectangular flat steel and employing a multi-pass rolling process, the instability problem in the rolling process of rectangular flat steel was solved, achieving high-precision and high-quality production of rectangular flat steel.
Patent Information
- Application Number
- CN202411163355.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
在扁钢轧制过程中,尤其是矩形扁钢的轧制过程中,存在高宽比大导致轧制不稳定、易脱方、扭转和疲劳裂纹的问题,难以控制尺寸和形状。
A rectangular flat steel pass design and rolling process is adopted, including multiple rolling processes such as continuous casting billet, heating, rough rolling, intermediate rolling, pre-finish rolling and finish rolling. By rationally designing pass parameters such as groove opening, groove bottom, inner round corner, and side wall slope, and combining with the cooling system to control the temperature and shape of the rolled piece, the stable deformation of the rolled piece in each pass and the high precision of the final product are ensured.
Stable rolling of rectangular flat steel was achieved, reducing torsion and desquamation, improving dimensional accuracy and surface quality, and ensuring product performance and quality stability.
Smart Images

Figure CN118904899A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flat steel processing, and in particular to a rectangular flat steel pass design and rolling process. Background Art
[0002] Spring steel includes 60Si2Mn, 50CrV4, 51CrV4, and 52CrMoV4, which are mainly used for automobiles. In recent years, with the upgrading of domestic enterprises' production equipment and the needs of the development of the automobile industry, the demand for spring steel has shown a rapid growth trend. At present, there are few domestic spring flat steel manufacturers, the price advantage of flat steel is obvious, and the market demand is large. It is estimated that the annual demand for spring flat steel will be 8 million tons from 2024 to 2025, and the demand for automobile spring flat steel will be about 3 million tons. It is well known that in the rolling process of flat steel, the aspect ratio of the rolled piece ≥1.5 is a stable state, and the closer it is to 1, the more unstable the rolling is, and it is very easy to have de-squareness, torsion of steel quality, and production accidents. The production of a 62mm*71mm rectangular flattened steel is very difficult and its size and shape are difficult to control. The reasons are: (1) The aspect ratio of the finished product size of 62mm*71mm is about 1.14, and the shape of the finished hole is similar to that of a box-shaped hole; (2) Due to the characteristics of the box-shaped hole structure, it is difficult to roll out square and rectangular cross-section rolled products with correct geometry and precise size from the box-shaped hole. The smaller the cross-section of the rolled product, the more serious this phenomenon is; (3) The arcs at the four corners of the finished product are small, and it is easy for the corners to be incomplete during the rolling process. At the same time, the r-angle is improperly designed, the stress is not released, there is stress concentration, and fatigue cracks are very likely to occur. Summary of the invention
[0003] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a rectangular flat steel hole design and rolling process that can solve the above-mentioned problem.
[0004] To achieve the above object, the present invention provides the following technical solutions: A rectangular flat steel pass design and rolling process, comprising the following specific steps: S1: continuous casting billet, first, injecting pretreated molten steel into the tundish of the continuous casting machine;
[0005] S2: Heating, placing the steel billet or ingot into a heating furnace for heating to reach a suitable rolling temperature;
[0006] S3: The rough rolling unit rolls the raw material of the billet through multiple rolling deformations, so that the thickness and width of the billet are gradually reduced, and the shape gradually approaches the preliminary shape required for the finished product;
[0007] S4: Head stripping temperature control stand. Head stripping refers to separating the head of the rolled piece from the main part for subsequent rolling or processing;
[0008] S5: rolling in the intermediate rolling mill. During the rolling process of the intermediate rolling mill, the workpiece after rough rolling enters the intermediate rolling mill. The number and layout of the rolling mills in the intermediate rolling mill are determined according to the production process and product requirements. At this stage, the workpiece is further deformed by rolling, the size gradually decreases, and the shape becomes more regular. The main process parameters in the rolling process include rolling speed, reduction, and rolling temperature;
[0009] S6: Pre-finishing mill rolling. During the pre-finishing mill rolling process, the rolled pieces from the intermediate mill enter the pre-finishing mill. Its main function is to further reduce the diameter of the rolled pieces and improve the dimensional accuracy, so as to provide intermediate billets with more accurate size and shape and better performance for the subsequent finishing mill. The pre-finishing mill usually consists of 2-6 rolling mills and adopts a torsion-free rolling method to reduce the torsion and bending of the rolled pieces during the rolling process, so as to ensure the dimensional accuracy and surface quality of the products.
[0010] S7: Finishing mill rolling. In the finishing mill rolling stage, the rolled pieces from the pre-finishing mill enter the finishing mill. The finishing mill usually consists of multiple rolling mills, usually 4-10. The layout of these rolling mills and the hole design of the rolls are accurately calculated and optimized to achieve high-precision rolling of the rolled pieces. During the rolling process, the rolling speed of the finishing mill is relatively high, usually reaching tens of meters per second. High-speed rolling helps to reduce the temperature drop of the rolled pieces during the rolling process and ensure that the rolled pieces are in a good plastic deformation state.
[0011] S8: Cooling on a cooling bed. After the rolling process is completed, the high-temperature rolled piece needs to be cooled on a cooling bed to reach the appropriate temperature and performance requirements.
[0012] Preferably, in the S3 process, the reduction is large: in order to achieve a larger deformation in a shorter rolling pass, the reduction in the rough rolling stage is usually larger;
[0013] The rolling speed is relatively low: Due to the large size of the billet and the large deformation resistance, the rolling speed is lower than that of the subsequent finishing stage;
[0014] High temperature: The temperature of the billet entering the rough rolling unit is high, and a large amount of heat will be generated during the rolling process, requiring effective cooling and temperature control measures.
[0015] Preferably, in the S4 process, in the rough rolling mill, after the workpiece has been rolled for multiple passes, the head may have irregular shape and uneven temperature, which may affect the quality and efficiency of subsequent rolling;
[0016] Through the head-stripping temperature-controlled stand, the head of the rolled piece can be cut off to separate it from the main part, and then the head can be processed separately, such as trimming, heating or cooling, to improve the quality of the rolled piece and the stability of rolling.
[0017] Preferably, in the S5 process, the rolling speed is adjusted in the intermediate rolling stage according to the deformation requirements of the rolled piece and the equipment capacity to ensure the quality and production efficiency of the rolled piece. The distribution of the reduction amount needs to comprehensively consider the material, size, temperature of the rolled piece and the requirements of the subsequent finishing rolling. Through reasonable reduction distribution, the rolled piece can achieve stable deformation and optimization of organizational properties in the intermediate rolling stage.
[0018] Preferably, in the S6 process, in terms of rolling technology, the rolling speed of the pre-finishing mill group is improved compared with the medium rolling mill group, and the hole design of the rolling roller is more sophisticated and complex to achieve accurate plastic deformation of the rolled piece, and the control of the rolling temperature is also very strict. Due to the generation of deformation heat and friction heat of the rolled piece during the rolling process, as well as heat exchange with the surrounding environment, the temperature of the rolled piece needs to be accurately controlled by the cooling system to ensure that the performance and structure of the rolled piece meet the requirements. At the same time, the equipment of the pre-finishing mill group is usually equipped with an advanced automatic control system for accurately adjusting rolling parameters, monitoring equipment operating status and ensuring the stability of product quality.
[0019] Preferably, in the S7 process, the reduction amount distribution of the finishing mill is relatively small, but the control requirements for dimensional accuracy and surface quality are extremely high. By accurately controlling the reduction amount, rolling force, rolling speed and roll gap parameters of each rolling mill, the dimensional accuracy of the rolled piece reaches the specified standard and the surface quality of the product is smooth and defect-free. In addition, temperature control during the finishing rolling process is also crucial. In order to ensure the performance and microstructure of the rolled piece, the cooling system needs to be used to accurately control the cooling of the rolled piece so that the rolled piece can obtain ideal structure and performance after leaving the finishing mill.
[0020] Preferably, in the S8 process, during the cooling process, on the one hand, the rolled material loses heat by heat radiation to the surrounding environment and heat convection with the air; on the other hand, some cooling beds are also equipped with forced cooling devices, such as air cooling or water cooling systems, to accelerate the cooling process of the rolled material. Through cooling on the cooling bed, the temperature of the rolled material can be evenly reduced, avoiding internal residual stress and structural unevenness caused by uneven cooling, thereby ensuring the performance and quality of the rolled material. In addition, cooling on the cooling bed can also straighten and fix the shape of the rolled material to a certain extent during the cooling process, reducing the bending and deformation of the rolled material.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The hole design and rolling process of the rectangular flat steel. The three-line special steel production line of this solution develops a 62mm*71mm rectangular spring flat made of 52CrMoV4 without changing the equipment. As a typical representative of domestic high-end spring flats, it has the advantages of high hardenability, low decarburization sensitivity and excellent mechanical processing performance. The company organized technical personnel to tackle the heating process, hole design, rolling process and slow cooling process, and successfully developed a 62mm*71mm rectangular spring flat steel made of 52CrMoV4 with stable quality, qualified performance and size that meets customer requirements.
[0023] 2. The hole design and rolling process of the rectangular flat steel. The hole design refers to the design and calculation work for the steel ingot or billet to be deformed by several rolling passes between two or more grooved rollers to obtain the product with the required cross-sectional shape, size and performance. The rationality of the design directly affects the quality of the product, the production capacity of the rolling mill, the cost of the product, the working conditions and the labor intensity. The hole design components include: groove, groove bottom, inner fillet, outer fillet, side wall slope, and roll gap geometric structure. The design of the groove bottom has an important influence on the stability of the rolled product and the product quality during the rolling process. A reasonable groove design will be beneficial to on-site process control and avoid the occurrence of ear defects. The fillet (R / r) can prevent the corner cracks caused by the rapid cooling of the corner of the rolled product and reduce the stress concentration at the corner. The side wall slope affects the stability of the rolled product and the product quality during the rolling process, and at the same time improves the life of the groove.
[0024] 3. The hole design and rolling process of the rectangular flat steel optimize the stability and fluidity of the flat steel during the vertical hole rolling process, reduce the torsion and de-squareness of the flat steel during the rolling process, and facilitate better control of the side shape and size of the flat steel during the rolling process. Combined with the gradual reduction of the inner fillet from 18mm to 14mm, it helps the flat steel to form a smoother rolling line shape during the rolling process, reduce stress concentration at the corners of the material, and avoid the occurrence of fatigue cracks at the corners. The design of gradually reducing the side wall slope and fillet can ensure that the rolled piece maintains a stable shape during the rolling process, reduce the risk of de-squareness and torsion, and improve the dimensional accuracy and surface quality of the rolled piece. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments:
[0026] Figure 1 This is a process flow chart of the three-line production of rods of the present invention;
[0027] Figure 2 This is a schematic diagram of the hole types of K6, K4 and K2 of the present invention;
[0028] Figure 3Schematic diagram of a 62mm*71mm rectangular 52CrMoV4 flattened carbon layer (left: corner, right: upper surface plane) of the present invention;
[0029] Figure 4 This is the metallographic structure diagram of the 62mm*71mm rectangular 52CrMoV4 flat spring of the present invention. DETAILED DESCRIPTION
[0030] This section will describe in detail the specific embodiments of the present invention. The preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the accompanying drawings is to supplement the description of the text part of the specification with graphics, so that people can intuitively and vividly understand each technical feature and the overall technical solution of the present invention, but it cannot be understood as a limitation on the scope of protection of the present invention.
[0031] In the description of the present invention, it should be understood that descriptions involving orientation, such as up, down, front, back, left, and right, and the orientation or positional relationship indicated are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0032] In the description of the present invention, "greater than", "less than" and "exceed" are understood as not including the number itself, and "above", "below" and "within" are understood as including the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0033] In the description of the present invention, unless otherwise clearly defined, the terms such as setting, installing and connecting should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention in combination with the specific content of the technical solution.
[0034] See also Figure 1-4 ,The present invention provides a technical solution: a rectangular flat steel pass design and rolling ,process, including the following specific steps, S1: continuous casting billet, first, the molten steel that has been pretreated (such as desulfurization, dephosphorization, and decarburization) is injected into the tundish of the continuous casting machine;
[0035] S2: Heating, placing the steel billet or ingot into a heating furnace for heating to reach a suitable rolling temperature;
[0036] S3: The rough rolling unit rolls the raw material of the billet through multiple rolling deformations, so that the thickness and width of the billet are gradually reduced, and the shape gradually approaches the preliminary shape required for the finished product;
[0037] Among them, the reduction is large: in order to achieve a larger deformation in a shorter rolling pass, the reduction in the rough rolling stage is usually larger;
[0038] The rolling speed is relatively low: Due to the large size of the billet and the large deformation resistance, the rolling speed is lower than that of the subsequent finishing stage;
[0039] High temperature: The temperature of the billet entering the rough rolling unit is high, and a large amount of heat will be generated during the rolling process, requiring effective cooling and temperature control measures;
[0040] S4: Head stripping temperature control stand. Head stripping refers to separating the head of the rolled piece from the main part for subsequent rolling or processing;
[0041] Among them, in the rough rolling unit, after multiple passes of rolling, the head of the rolled piece may have irregular shape and uneven temperature, which affects the quality and efficiency of subsequent rolling;
[0042] Through the head-stripping temperature-control stand, the head of the rolled piece can be cut off to separate it from the main part, and then the head can be processed separately, such as trimming, heating or cooling, to improve the quality of the rolled piece and the stability of rolling;
[0043] S5: rolling in the intermediate rolling mill. During the rolling process of the intermediate rolling mill, the workpiece after rough rolling enters the intermediate rolling mill. The number and layout of the rolling mills in the intermediate rolling mill are determined according to the production process and product requirements. At this stage, the workpiece is further deformed by rolling, the size gradually decreases, and the shape becomes more regular. The main process parameters in the rolling process include rolling speed, reduction, and rolling temperature;
[0044] Among them, the rolling speed will be adjusted in the intermediate rolling stage according to the deformation requirements of the rolled piece and the equipment capacity to ensure the quality and production efficiency of the rolled piece. The distribution of the reduction amount needs to comprehensively consider the material, size, temperature of the rolled piece and the requirements of the subsequent finishing rolling. Through reasonable reduction distribution, the rolled piece can achieve stable deformation and optimization of organizational properties in the intermediate rolling stage;
[0045] S6: Pre-finishing mill rolling. During the pre-finishing mill rolling process, the rolled pieces from the intermediate mill enter the pre-finishing mill. Its main function is to further reduce the diameter of the rolled pieces and improve the dimensional accuracy, so as to provide intermediate billets with more accurate size and shape and better performance for the subsequent finishing mill. The pre-finishing mill usually consists of 2-6 rolling mills and adopts a torsion-free rolling method to reduce the torsion and bending of the rolled pieces during the rolling process, so as to ensure the dimensional accuracy and surface quality of the products.
[0046] Among them, in terms of rolling process, the rolling speed of the pre-finishing mill is higher than that of the medium rolling mill, and the hole design of the roll is more sophisticated and complex to achieve precise plastic deformation of the rolled piece. The control of the rolling temperature is also very strict. Due to the generation of deformation heat and friction heat of the rolled piece during the rolling process, as well as heat exchange with the surrounding environment, the temperature of the rolled piece needs to be accurately controlled through the cooling system to ensure that the performance and organization of the rolled piece meet the requirements. At the same time, the equipment of the pre-finishing mill is usually equipped with an advanced automatic control system for accurately adjusting rolling parameters, monitoring equipment operating status and ensuring the stability of product quality.
[0047] S7: Finishing mill rolling. In the finishing mill rolling stage, the rolled pieces from the pre-finishing mill enter the finishing mill. The finishing mill usually consists of multiple rolling mills, usually 4-10. The layout of these rolling mills and the hole design of the rolls are accurately calculated and optimized to achieve high-precision rolling of the rolled pieces. During the rolling process, the rolling speed of the finishing mill is relatively high, usually reaching tens of meters per second. High-speed rolling helps to reduce the temperature drop of the rolled pieces during the rolling process and ensure that the rolled pieces are in a good plastic deformation state.
[0048] The reduction distribution of the finishing mill is relatively small, but the control requirements for dimensional accuracy and surface quality are extremely high. By accurately controlling the reduction, rolling force, rolling speed and roll gap parameters of each rolling mill, the dimensional accuracy of the rolled piece can reach the specified standard, and the surface quality of the product can be smooth and defect-free. In addition, temperature control during the finishing rolling process is also crucial. In order to ensure the performance and microstructure of the rolled piece, the cooling system needs to be used to accurately control the cooling of the rolled piece so that the rolled piece can obtain the ideal structure and performance after leaving the finishing mill.
[0049] S8: Cooling on a cooling bed. After the rolling process is completed, the high-temperature rolled piece needs to be cooled on a cooling bed to reach the appropriate temperature and performance requirements.
[0050] Among them, during the cooling process, on the one hand, the rolled material loses heat through heat radiation to the surrounding environment and heat convection with the air; on the other hand, some cooling beds are also equipped with forced cooling devices, such as air cooling or water cooling systems, to accelerate the cooling process of the rolled material. Through cooling on the cooling bed, the temperature of the rolled material can be evenly reduced, avoiding internal residual stress and uneven structure problems caused by uneven cooling, thereby ensuring the performance and quality of the rolled material. In addition, cooling on the cooling bed can also straighten and fix the shape of the rolled material to a certain extent during the cooling process, reducing the bending and deformation of the rolled material.
[0051] Furthermore, the chemical composition of 52CrMoV4 steel
[0052] The 52CrMoV4 continuous casting billet with a cross section of 280mm*280mm produced by the five-meter wide and thick plate continuous casting workshop of Xiangtan Steel was selected. The chemical composition was controlled according to the technical requirements. The specific content of each element is shown in Table 1 below.
[0053] Table 1 Chemical composition of 52CrMoV4
[0054]
[0055] Heating process and slow cooling process
[0056] In order to avoid the influence of different heating temperatures on the performance of 52CrMoV4 steel, the heating temperature and furnace time in this paper are strictly controlled according to Table 2. The residual oxygen content of the steel after entering the furnace is controlled to be ≤2% throughout the whole process. The furnace is slightly positively pressurized, the upper cooling bed temperature is 750±20℃, and the slow cooling speed is controlled by the opening angle of the insulation cover and the steel layout of the cooling bed to be 0.5-2℃ / s.
[0057] Table 2 Heating temperature and furnace schedule
[0058]
[0059] Results and Analysis
[0060] Hole design
[0061] Pass design refers to the process of rolling an ingot or billet between two or more grooved rolls for several times to obtain a product with the required cross-sectional shape, size and performance. The design and calculation work for this purpose directly affects the quality of the product, the production capacity of the rolling mill, the cost of the product, the working conditions and the intensity of the labor. The pass design components include: notch, groove bottom, inner fillet, outer fillet, side wall slope, and roll gap geometry. The design of the groove bottom has an important influence on the stability of the rolled product and the product quality during the rolling process. A reasonable notch design will be beneficial to on-site process control and avoid the occurrence of ear defects. The fillet (R / r) can prevent the corner cracks caused by the rapid cooling of the corner of the rolled product and reduce the stress concentration at the corner. The side wall slope affects the stability of the rolled product and the product quality during the rolling process, and at the same time improves the life of the groove. According to the national standard GBT As shown in 33164.1-2016 Spring steel for automobile suspension system Part 1: Hot rolled flat steel, the national standard finished product r angle of 62mm*71mm rectangular flat steel is 12mm±2mm, the allowable deviation thickness of group 1 is ±0.4mm, and the width is ±0.6mm. The hole type of 62mm*71mm rectangular flat steel is as follows Figure 2As shown, the groove bottom design of K2 is 64.00mm, the groove design is 79.19mm, the R angle design is R14mm, the side wall slope is 5°, the groove depth is 30.5mm, and the roller gap is 10mm; the groove bottom design of K4 is 63.00mm, the groove design is 70.32mm, the R angle design is R16mm, the side wall slope is 6°, the groove depth is 35mm, and the roller gap is 20mm; the groove bottom design of K6 is 69mm, the groove design is 77.59mm, the R angle design is R18mm, the side wall slope is 7°, the groove depth is 35mm, and the roller gap is 20mm. The side wall slope of K6-K4-K2 The gradual reduction from 7° to 5° optimizes the stability and fluidity of the flat steel during the vertical hole rolling process, reduces the torsion and de-squareness of the flat steel during the rolling process, and facilitates better control of the side shape and size of the flat steel during the rolling process. Combined with the gradual reduction of the inner fillet from 18mm to 14mm, it helps the flat steel to form a smoother rolling line shape during the rolling process, reduce the stress concentration at the corners of the material, and avoid the occurrence of fatigue cracks at the corners. The design of gradually reducing the side wall slope and fillet can ensure that the rolled piece maintains a stable shape during the rolling process, reduce the risk of de-squareness and torsion, and improve the dimensional accuracy and surface quality of the rolled piece;
[0062] Furthermore, the rolling schedule
[0063] The rolling schedule is a key tool in steel rolling production. It plans the rolling process parameters in detail, such as rolling speed, rolling reduction, and rolling passes. By reasonably arranging the rolling sequence and process parameters, the rolling process can be optimized, production efficiency can be improved, and production costs can be reduced. The 62mm*71mm rectangular spring flat rolling schedule is shown in Table 3. There are a total of 20 rolling mills, of which the first 10 use a box-elliptical-circular hole system, 10 produce semi-finished rounds with a diameter of 112.5mm, and 1-4 rolling mills are box-type hole systems. Through their large reduction and hole commonality, the rolled pieces can be quickly rolled to a certain size and shape. The cross-section of the 52CrMoV4 continuous casting billet is 280mm*280mm , the reduction amounts of 1-4 stands are 52mm, 66mm, 63mm, and 57.5mm respectively. The larger reduction amount can improve the density of the flat steel, eliminate the pores inside the material, and at the same time obtain finer grains, improve the internal quality of the material and improve the overall performance. 1-4 stands adopt a box-type hole system with large hole commonality. This system can share billets with sections of 150mm*150mm, 240mm*240mm, and 280mm*280mm without changing the rolling mill, thereby improving production efficiency. 5-10 stands are elliptical-circular hole systems with the advantages of uniform deformation, good surface quality, and stable process. The design of the elliptical-circular hole system ensures the uniformity of the deformation of the rolled piece and avoids It avoids local stress caused by severe uneven deformation of rolled pieces and reduces cracks and other surface defects caused by uneven cooling. At the same time, the rolled pieces rolled out by the elliptical-circular hole system have no sharp edges and corners, and the smooth shape helps to improve the surface quality of the rolled pieces. The 11th frame starts with a flat roll with a rectangular vertical hole hole (K6 / K4 / K2), where the reduction of K6, K4, and K2 is 27mm, 19mm, and 13.5mm respectively. The reduction of the special vertical hole is gradually reduced, which is conducive to the filling of the r corner of the flat steel, so that the flat steel corner meets 14mm. At the same time, the aspect ratios of K6, K4, and K2 rolled pieces are 1.31, 1.20, and 1.03 respectively. The rolled pieces tend to be more unstable. In order to avoid the unstable state caused In order to prevent the torsion, add a flat roller between the special vertical holes of K6 and K4 and add a certain amount of reduction (K6 is reduced by 34mm and K4 is reduced by 19mm), which can reduce the lateral expansion during the rolling process, making the rolled piece more stable during the rolling process, and reducing the occurrence of the problem of the rolled piece running off and twisting. At the same time, the opening of the rolling mill guides corresponding to K6, K4 and K2 is set to be consistent with the rolled piece, and the guides are in the two-way rolling mill of the rolling mill, so as to avoid the torsion and steel piling of the rolled piece. At the same time, it can be seen from Table 3 that 12V and 20V are both empty, which can facilitate the replacement of the other rolling mills in case of failure, quickly resume production and improve production efficiency; the reduction of the 19 finished flat rollers is less than 10mm, and the smaller reduction is conducive to ensuring the shape of the side and r angle of the finished product.
[0064] Combination Figure 2 K6, K4, K2 hole diagram and Table 3 62mm*71mm rectangular flat steel rolling program table, the rolled material between K6, K4, K2 is evenly distributed between the groove bottom and the groove mouth, which is beneficial to the uniformity of rolled deformation and rolling force distribution, and further avoids the occurrence of torsion.
[0065] Table 3 62mm*71mm rectangular flat steel rolling schedule
[0066]
[0067] Decarbonization analysis
[0068] Decarburization of spring steel refers to the behavior of reducing carbon atoms on the surface of unoxidized steel, which is divided into partial decarburization and full decarburization. Its fatigue life decreases with the increase of decarburization layer. When a complete decarburization layer appears on the surface of spring steel, the fatigue limit will be reduced by about 50%. Therefore, to increase the service life of the spring, it is necessary to reduce the depth of the decarburization layer and avoid the formation of a complete decarburization layer. All samples are cut, ground and polished, and then corroded with 4% nitric acid alcohol (volume ratio) solution. The microstructure of the polished surface is observed by metallographic method. The deepest decarburization is taken as the depth of the decarburization layer. The depth of the flat carbon layer of 62mm*71mm rectangular 52CrMoV4 spring is as follows: Figure 3 As shown in the figure, it can be seen that the surface is a partial decarburized layer of reticular ferrite, and no complete decarburized layer appears. The depth of the decarburized layer at the arc position of the decarburized layer is about 0.28mm ( Figure 3 Left), the straight edge decarburization layer depth is 0.26mm ( Figure 3 Right), according to research, higher carbon content in spring steel, higher heating temperature in the heating furnace, longer heating time and strong oxidizing heating medium will increase the thickness of the decarburized layer, while the lower heating process and lower oxidizing gas in the furnace of Xianggang Rod Line 3 are conducive to reducing the depth of the decarburized layer on the surface of spring steel and avoiding the formation of a complete decarburized layer. At the same time, Xianggang Rod Line 3 continues to reduce the depth of the decarburized layer by reducing the oxidizing gases H2O, CO2, and O2 in the heating furnace, such as controlling the residual oxygen content ≤1% and using coal gas dehydration methods to provide customers with products with better performance.
[0069] Furthermore, hot rolling hardness analysis
[0070] The upper cooling bed temperature of 62mm*71mm rectangular 52CrMoV4 flattened was controlled to be 750±20℃, and the slow cooling speed was controlled to be 0.5℃ / s, 1℃ / s and 2℃ / s respectively. The influence of different slow cooling speeds on the mechanical properties of the product was studied. Points were made in the center area of the sample, 20 points were made for each sample, and each point was separated by an appropriate distance. The average hardness value was taken. Table 4 shows the hot-rolled hardness value of 62mm*71mm rectangular 52CrMoV4 flattened at different slow cooling speeds. It can be found from the table that the hot-rolled hardness value of the flattened product is proportional to the slow cooling rate. The lower the slow cooling speed, the lower the hot-rolled hardness value. When the slow cooling speed is 0.5℃ / s, 1℃ / s and 2℃ / s, the hot-rolled hardness is 310HB, 348HB and 409HB respectively. Figure 4 The metallographic images of 62mm*71mm rectangular 52CrMoV4 flattened at slow cooling rates of 0.5℃ / s (a), 1℃ / s (b) and 2℃ / s (c) are shown in Figure 1. Figure 4 It is found that the matrix structure of (a / b) is mainly troostite + pearlite + a small amount of ferrite; the matrix structure of (c) is troostite + pearlite + a small amount of residual martensite + a small amount of ferrite. Figure 4 According to the analysis, when the cooling rate is fast (2℃ / s), the microstructure after phase transformation is more inclined to form martensite, which is a hard and brittle phase, so it will increase the hardness of the flattening. When the slow cooling rate is low (<1℃ / s), the phase transformation microstructure is more inclined to form pearlite or ferrite, which is softer than martensite. These microstructures have lower hardness than martensite. Therefore, in order to obtain lower hot-rolled hardness and reduce customer processing costs, the slow cooling rate of 62mm*71mm rectangular 52CrMoV4 flattening should be controlled to be less than 0.5℃ / s.
[0071] Table 4 Hot rolling hardness values of 62mm*71mm rectangular 52CrMoV4 flattened at different slow cooling rates
[0072]
[0073] See also Figure 4 , a slow cooling rate 0.5℃ / s; b slow cooling rate 1℃ / s; c slow cooling rate 2℃ / s, Conclusion
[0074] 1. The groove bottom design of K2 is 64.00mm, the groove design is 79.19mm, the R angle design is R14mm, the side wall slope is 5°, the groove depth is 30.5mm, and the roll gap is 10mm; the groove bottom design of K4 is 63.00mm, the groove design is 70.32mm, the R angle design is R16mm, the side wall slope is 6°, the groove depth is 35mm, and the roll gap is 20mm; the groove bottom design of K6 is 69mm, the groove design is 77.59mm, the R angle design is R18mm, the side wall slope is 7°, the groove depth is 35mm, and the roll gap is 20mm;
[0075] 2. The side wall slope of K6-K4-K2 is gradually reduced from 7° to 5°, and the fillet is gradually reduced from 18mm to 14mm, which can better control the side shape and size of the flat steel during the rolling process, reduce the torsion and squareness of the flat steel during the rolling process, and reduce the stress concentration at the corners of the material to avoid the occurrence of fatigue cracks at the corners;
[0076] 3. The aspect ratios of K6, K4 and K2 rolled products are 1.31, 1.20 and 1.03 respectively. Flat rolls are added between the special vertical holes of K6 and K4, and a certain amount of reduction is added (34mm for K6 and 19mm for K4) to reduce the lateral width expansion during the rolling process, making the rolled products more stable during the rolling process and reducing the occurrence of deviation and torsion problems of the rolled products.
[0077] 4. 62mm*71mm rectangular 52CrMoV4 flat spring has no complete decarburization layer, and the depth of decarburization layer is 0.26-0.28mm;
[0078] 5. The hot-rolled hardness value of 62mm*71mm rectangular 52CrMoV4 flattened steel is proportional to the slow cooling rate. The lower the slow cooling rate, the lower the hot-rolled hardness value. When the slow cooling rate is 0.5℃ / s, 1℃ / s and 2℃ / s, the hot-rolled hardness is 310HB, 348HB and 409HB respectively.
[0079] 6. The matrix structure of the slow cooling rate of 0.5℃ / s and 1℃ / s is mainly troostite + pearlite + a small amount of ferrite, and the slow cooling rate of 2℃ / s is troostite + pearlite + a small amount of residual martensite + a small amount of ferrite.
[0080] Furthermore, without changing the equipment, the three-line special steel production line of this plan developed a 62mm*71mm rectangular spring flat made of 52CrMoV4. As a typical representative of domestic high-end spring flats, it has the advantages of high hardenability, low decarburization sensitivity and excellent mechanical processing performance. The company organized technical personnel to tackle the heating process, hole design, rolling process and slow cooling process, and successfully developed a 62mm*71mm rectangular spring flat steel made of 52CrMoV4 with stable quality, qualified performance and size that meets customer requirements.
[0081] The embodiments of the present invention are described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the technical field without departing from the purpose of the present invention.
Claims
1. A rectangular flat steel pass design and rolling process, characterized in that: The method comprises the following specific steps: S1: continuously casting a billet, firstly, injecting the pre-treated molten steel into a tundish of a continuous casting machine; S2: Heating, placing the steel billet or ingot into a heating furnace for heating to reach a suitable rolling temperature; S3: The rough rolling unit rolls the raw material of the billet through multiple rolling deformations, so that the thickness and width of the billet are gradually reduced, and the shape gradually approaches the preliminary shape required for the finished product; S4: Head stripping temperature control stand. Head stripping refers to separating the head of the rolled piece from the main part for subsequent rolling or processing; S5: rolling in the intermediate rolling mill. During the rolling process of the intermediate rolling mill, the workpiece after rough rolling enters the intermediate rolling mill. The number and layout of the rolling mills in the intermediate rolling mill are determined according to the production process and product requirements. At this stage, the workpiece is further deformed by rolling, the size gradually decreases, and the shape becomes more regular. The main process parameters in the rolling process include rolling speed, reduction, and rolling temperature; S6: Pre-finishing mill rolling. During the pre-finishing mill rolling process, the rolled pieces from the intermediate mill enter the pre-finishing mill. Its main function is to further reduce the diameter of the rolled pieces and improve the dimensional accuracy, so as to provide intermediate billets with more accurate size and shape and better performance for the subsequent finishing mill. The pre-finishing mill usually consists of 2-6 rolling mills and adopts a torsion-free rolling method to reduce the torsion and bending of the rolled pieces during the rolling process, so as to ensure the dimensional accuracy and surface quality of the products. S7: Finishing mill rolling. In the finishing mill rolling stage, the rolled pieces from the pre-finishing mill enter the finishing mill. The finishing mill usually consists of multiple rolling mills, usually 4-10. The layout of these rolling mills and the hole design of the rolls are accurately calculated and optimized to achieve high-precision rolling of the rolled pieces. During the rolling process, the rolling speed of the finishing mill is relatively high, usually reaching tens of meters per second. High-speed rolling helps to reduce the temperature drop of the rolled pieces during the rolling process and ensure that the rolled pieces are in a good plastic deformation state. S8: Cooling on a cooling bed. After the rolling process is completed, the high-temperature rolled piece needs to be cooled on a cooling bed to reach the appropriate temperature and performance requirements.
2. A rectangular flat steel pass design and rolling process according to claim 1, characterized in that: In the S3 process, the reduction is large: in order to achieve a larger deformation in a shorter rolling pass, the reduction in the rough rolling stage is usually larger; The rolling speed is relatively low: Due to the large size of the billet and the large deformation resistance, the rolling speed is lower than that of the subsequent finishing stage; High temperature: The temperature of the billet entering the rough rolling unit is high, and a large amount of heat will be generated during the rolling process, requiring effective cooling and temperature control measures.
3. The rectangular flat steel pass design and rolling process according to claim 1, characterized in that: During the S4 process, in the rough rolling mill, after the workpiece has been rolled for multiple passes, the head may have irregular shapes and uneven temperatures, which may affect the quality and efficiency of subsequent rolling. Through the head-stripping temperature-controlled stand, the head of the rolled piece can be cut off to separate it from the main part, and then the head can be processed separately, such as trimming, heating or cooling, to improve the quality of the rolled piece and the stability of rolling.
4. The rectangular flat steel pass design and rolling process according to claim 1, characterized in that: In the S5 process, the rolling speed will be adjusted in the intermediate rolling stage according to the deformation requirements of the rolled piece and the equipment capacity to ensure the quality and production efficiency of the rolled piece. The distribution of the reduction amount needs to comprehensively consider the material, size, temperature of the rolled piece and the requirements of subsequent finishing rolling. Through reasonable reduction distribution, the rolled piece can achieve stable deformation and optimization of organizational properties in the intermediate rolling stage.
5. The rectangular flat steel pass design and rolling process according to claim 1, characterized in that: In the S6 process, in terms of rolling technology, the rolling speed of the pre-finishing mill is higher than that of the medium rolling mill, and the hole design of the rolls is more sophisticated and complex to achieve accurate plastic deformation of the rolled piece. The control of the rolling temperature is also very strict. Due to the generation of deformation heat and friction heat of the rolled piece during the rolling process, as well as heat exchange with the surrounding environment, the temperature of the rolled piece needs to be accurately controlled by the cooling system to ensure that the performance and organization of the rolled piece meet the requirements. At the same time, the equipment of the pre-finishing mill is usually equipped with an advanced automatic control system for accurately adjusting rolling parameters, monitoring equipment operation status and ensuring the stability of product quality.
6. The rectangular flat steel pass design and rolling process according to claim 1, characterized in that: In the S7 process, the reduction amount of the finishing mill is relatively small, but the control requirements for dimensional accuracy and surface quality are extremely high. By accurately controlling the reduction amount, rolling force, rolling speed and roll gap parameters of each rolling mill, the dimensional accuracy of the rolled piece reaches the specified standard, and the surface quality of the product is smooth and defect-free. In addition, temperature control during the finishing rolling process is also crucial. In order to ensure the performance and microstructure of the rolled piece, the cooling system needs to be used to accurately control the cooling of the rolled piece so that the rolled piece can obtain ideal structure and performance after leaving the finishing mill.
7. The rectangular flat steel pass design and rolling process according to claim 1, characterized in that: In the S8 process, during the cooling process, on the one hand, the rolled material loses heat by heat radiation to the surrounding environment and heat convection with the air; on the other hand, some cooling beds are also equipped with forced cooling devices, such as air cooling or water cooling systems, to accelerate the cooling process of the rolled material. Through cooling on the cooling bed, the temperature of the rolled material can be evenly reduced, avoiding internal residual stress and structural unevenness caused by uneven cooling, thereby ensuring the performance and quality of the rolled material. In addition, cooling on the cooling bed can also straighten and fix the shape of the rolled material to a certain extent during the cooling process, reducing the bending and deformation of the rolled material.
Citation Information
Patent Citations
Rolling and cooling method for flat spring steel
CN112893490A
Rolling method of plane rectangular spring flat steel
CN116651926A
Rectangular flat steel pass design and rolling process
CN117943418A
Compact bar production line and high-quality special steel bar production method
CN118237396A
Spring steel having superior fatigue life, and manufacturing method for same
WO2020020066A1
Cited By
Rolling method for enabling size of bar to exceed one set of precision
CN119346628A
A method for rolling a bar to a size beyond a set of precision
CN119346628B