Cold rolling pressure processing method for non-oriented silicon steel product
By adopting specific cold rolling pressure processing methods in the cold rolling process of non-oriented silicon steel, controlling the rolling parameters and lubrication and cooling process, the problems of poor stability and low yield of high-silicon and high-aluminum materials in the cold rolling process are solved, and the problem of low yield of high-silicon and high-aluminum materials in the cold rolling process is achieved. High quality and high efficiency rolling effect.
Patent Information
- Application Number
- CN202310499668.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Non-oriented silicon steel products have problems of poor stability and low yield during cold rolling, especially in high silicon and high alumina materials, which leads to high rolling difficulty and low efficiency.
Using specific cold rolling pressure processing methods, including primary cold rolling and secondary cold rolling steps, ensure plate shape accuracy and surface quality by controlling rolling passes, pressure ratio, tension and lubrication cooling processes, using different concentrations and temperatures The emulsion is lubricated and cooled, and a low roughness working roller is used in the secondary cold rolling step to improve product stability.
The rolling stability and yield of non-oriented silicon steel products are improved, the high-quality and efficient rolling process is ensured, and the transverse stripe defects and plate shape failure rate of the strip surface after rolling is reduced.
Smart Images

Figure CN118904909A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a steel plate, and in particular to a cold rolling process for silicon-free steel. Background Art
[0002] At present, non-oriented silicon steel products are widely used in electric motors, which have high requirements for product strength and magnetic induction. In order to meet the performance requirements, non-oriented silicon steel products often need to increase the Si+Al ratio of the product to 3.5%-5.0%, and control the normalizing annealing temperature at 900-1000℃ to ensure that the performance level meets the requirements. More importantly, cold rolling is required.
[0003] By adopting the cold rolling pressure processing method, after the first cold rolling, the stress is eliminated after recrystallization annealing at 900-1000℃, and a better grain structure can be obtained. After the second cold rolling, the magnetic properties of the product can be greatly improved and the iron loss can be reduced. Therefore, compared with the products formed by one cold rolling, multiple cold rolling has more advantages.
[0004] Based on this, it is desired to provide a cold rolling pressure processing method for non-oriented silicon steel products, which further improves the performance of non-oriented silicon steel by designing and improving the cold rolling process. Summary of the invention
[0005] The object of the present invention is to provide a cold rolling pressure processing method for non-oriented silicon steel products, which ensures the stability of the cold rolling process through the specific design of the cold rolling process to obtain better plate shape accuracy and surface quality, thereby improving the performance of the non-oriented silicon steel products.
[0006] In order to achieve the above object, the present invention provides a cold rolling pressure processing method for non-oriented silicon steel products, which includes a primary cold rolling step and a secondary cold rolling step, wherein:
[0007] In the first cold rolling step: a single-stand rolling mill is used for reciprocating rolling, and a first-rolled intermediate strip is formed through 3-5 passes, wherein the rolling reduction rate of each pass is controlled between 17-38%, and the entrance tension of each pass is controlled between 50-150N / mm 2 The exit tension of each rolling pass is controlled at 120-220N / mm 2 ; And during the rolling process, the strip is lubricated and cooled with emulsion so that the strip outlet temperature of the first pass is 120-200℃, and the strip outlet temperature of the 2nd to 5th pass is 70-120℃;
[0008] In the secondary cold rolling step: a single-stand rolling mill is used for reciprocating rolling, and the product thickness is reached through an even number of passes, wherein the reduction rate of each pass is controlled to be 30%-45%, and the entrance tension of each pass is controlled to be 90-180N / mm2 The exit tension of each rolling pass is controlled at 160-260N / mm 2 ; And during the rolling process, emulsion is used to lubricate and cool the strip so that the strip outlet temperature is 50-75℃.
[0009] For the high-silicon and high-aluminum steel used in new energy vehicles, the total mass percentage of Al and Si reaches 3.5%-5.0%. After regular pickling and high-temperature annealing at 850-1000℃, the number of rebending times at room temperature is very low. Therefore, the rollability of the product itself is very challenging, the rolling difficulty is high, and the rolling product rate is low.
[0010] In addition, this product undergoes intermediate annealing at 800-1100℃ after rolling, and its strength and other characteristics change significantly after recrystallization. Although nitrogen and hydrogen protective gases are used in the annealing process, there is a significant difference between the surface of the strip and the surface of the original first rolled strip, and there is an oxide layer, which will also have a significant impact on the stability of the second rolling.
[0011] In order to solve this problem, the present invention utilizes appropriate pass control, reduction rate control and tension process control in the first cold rolling and second cold rolling steps, and controls the plate temperature through lubrication cooling, thereby solving the problems of poor stability and low yield of high-silicon and high-aluminum products in the first rolling; ensuring the high quality, high stability and high rolling efficiency of the products during the second cold rolling. Among them, the pass reduction rate of the second cold rolling is controlled at 30%-45%, which can ensure a certain rolling force to avoid the uncontrollable plate shape caused by too small rolling force. The entrance tension during the second cold rolling pass is controlled at 90-180N / mm 2 ;Export tension is controlled at 160-260N / mm 2 The appropriate plate shape can be guaranteed, and there will be no transverse stripe defects on the surface of the strip after re-rolling.
[0012] Furthermore, in the cold rolling pressure processing method of the present invention, in a cold rolling step, lubricating and cooling the steel strip with an emulsion specifically includes:
[0013] In the first pass, the strip cooling nozzles at the rolling pass entrance, the strip cooling nozzles at the rolling pass exit, and the roll gap lubrication cooling nozzles at the rolling pass exit are all closed, and the roll gap lubrication cooling nozzles at the rolling pass entrance are opened;
[0014] In the 2nd to 5th passes, the strip cooling nozzles at the rolling pass entrance and the strip cooling nozzles at the rolling pass exit are controlled to be closed, and the roll gap lubrication cooling nozzles at the rolling pass exit and the roll gap lubrication cooling nozzles at the rolling pass entrance are controlled to be opened.
[0015] Furthermore, in the cold rolling pressure processing method described in the present invention, in the secondary cold rolling step, the use of emulsion to lubricate and cool the steel strip specifically includes: controlling the strip cooling nozzle at the entrance of the rolling pass, the strip cooling nozzle at the exit of the rolling pass, the roll gap lubrication cooling nozzle at the exit of the rolling pass, and the roll gap lubrication cooling nozzle at the entrance of the rolling pass to be open.
[0016] That is to say, in a cold rolling step, the first pass uses an emulsion to lubricate and cool the strip in a high-temperature mode; the subsequent 2-5 passes use a medium-temperature mode; and in the secondary cold rolling step, a low-temperature mode is used.
[0017] Furthermore, in the cold rolling pressure processing method described in the present invention, in a cold rolling step, a working roll with a roughness of 1.0-2.5 μm is used for rolling.
[0018] In a cold rolling step, the use of the above-mentioned high-roughness working rolls for rolling can effectively avoid slippage of the rolled plate and strip.
[0019] Furthermore, in the cold rolling pressure processing method of the present invention, in the secondary cold rolling step, a working roll with a roughness of 0.1-0.5 μm is used for rolling.
[0020] During the secondary cold rolling, the surface quality of the final strip steel can be ensured by using the above-mentioned low-roughness working rolls for rolling.
[0021] Furthermore, in the cold rolling pressure processing method described in the present invention, in a primary cold rolling step, a normalized pickled strip with a thickness of 1.5-2.4 mm is rolled into a primary rolled intermediate strip with a thickness of 0.5-0.7 mm.
[0022] Furthermore, in the cold rolling pressure processing method of the present invention, in a cold rolling step, the temperature of the emulsion is 50-70° C.; and / or the mass percentage concentration of the emulsion is 5-8%.
[0023] Furthermore, in the cold rolling pressure processing method of the present invention, in a cold rolling step, the temperature of the emulsion is 50-70° C.; and / or the mass percentage concentration of the emulsion is 3-8%.
[0024] Preferably, the concentration of the emulsion used in the first cold rolling step is higher than that of the emulsion used in the second cold rolling step.
[0025] Furthermore, in the cold rolling pressure processing method described in the present invention, in the secondary cold rolling step, the number of rolling passes is 2 or 4.
[0026] Furthermore, in the cold rolling pressure processing method of the present invention, before the first cold rolling step, a leader strip with a length of 5-20m is welded at the head and tail of the plate strip.
[0027] The leader can be made of medium or low grade scrap rolls or waste rolls from related work. Using the leader can reduce the loss of genuine products and increase the yield rate of genuine products.
[0028] Furthermore, in the cold rolling pressure processing method described in the present invention, there is an intermediate annealing step between the primary cold rolling step and the secondary cold rolling step, and a sleeve is provided at the exit coiler of the annealing unit in the intermediate annealing step.
[0029] In order to prevent the coil collapse phenomenon caused by rolling thinner products, the present invention can add a sleeve to the annealing unit outlet coiler when performing the intermediate annealing step between the primary cold rolling step and the secondary cold rolling step, so as to reduce the problem of low efficiency of the single-stand rolling mill caused by the need to add the sleeve when rolling on the single-stand rolling mill.
[0030] Furthermore, the cold rolling pressure processing method of the present invention is used for non-oriented silicon steel products with a mass percentage of Si+Al of 3.5-5.0%.
[0031] Furthermore, in the cold rolling pressure processing method described in the present invention, the finished product thickness is 0.15-0.3 mm.
[0032] Furthermore, in the cold rolling pressure processing method described in the present invention, the normalized pickled strip is heated before the first cold rolling step.
[0033] In some embodiments, an electromagnetic induction device may be used to heat the normalized pickled strip.
[0034] Furthermore, the heating temperature is 100-150°C.
[0035] This heating step can ensure that the strip has good plasticity and at the same time make the heating uniformity in the width direction of the strip better, thereby improving the rollability of the product.
[0036] The cold rolling pressure processing method for non-oriented silicon steel products of the present invention has the following advantages and beneficial effects:
[0037] The cold rolling pressure processing method of the present invention is applicable to high-silicon and high-aluminum non-oriented silicon steel products. It solves the problems of poor stability and low rolling yield rate during the rolling process through a specific primary cold rolling process and a lubrication cooling process. At the same time, it ensures high quality, high stability and high rolling efficiency of the product during the secondary rolling through a specific secondary cold rolling process and a lubrication cooling process. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 A flow chart showing the steps of the cold rolling pressure processing method according to some embodiments of the present invention.
[0039] Figure 2 A schematic diagram of the emulsion injection control of the first pass in a cold rolling step in some embodiments of the cold rolling pressure processing method described in the present invention is shown.
[0040] Figure 3 A schematic diagram showing emulsion injection control for 2-5 passes in a cold rolling step in some embodiments of the cold rolling pressure processing method of the present invention is shown.
[0041] Figure 4 A schematic diagram of emulsion injection control in the secondary cold rolling step of the cold rolling pressure processing method according to some embodiments of the present invention is shown. DETAILED DESCRIPTION
[0042] The cold rolling pressure processing method for non-oriented silicon steel products described in the present invention will be further explained and illustrated below in conjunction with specific embodiments and the accompanying drawings of the specification. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.
[0043] Figure 1 A flow chart showing the steps of the cold rolling pressure processing method according to some embodiments of the present invention.
[0044] like Figure 1 As shown, in some embodiments, the cold rolling pressure processing method for non-oriented silicon steel products comprises the steps of:
[0045] 100: Get the normalized pickled strip.
[0046] In some more specific embodiments, the normalized pickled plate has a thickness of 1.5-2.4 mm.
[0047] 200: Weld 5-20m long guide strips at the head and tail of the normalized pickled plate to improve the yield rate of genuine products.
[0048] 300: Using an electromagnetic induction device to heat the normalized pickled strip. In some more specific embodiments, the heating temperature is 100-150°C.
[0049] 400: Single cold rolling: A single-stand rolling mill is used for reciprocating rolling, and a single-rolled intermediate plate with a thickness of 0.5-0.7mm is rolled through 3-5 passes, wherein the rolling reduction rate of each pass is controlled between 17-38%, and the entrance tension of each pass is controlled to be 50-150N / mm 2The exit tension of each rolling pass is controlled at 120-220N / mm 2 ; and in the rolling process, in the first pass, an emulsion with a mass percentage concentration of 5-8% and a temperature of 50-70°C is used to lubricate and cool the strip in a "high temperature mode" so that the strip outlet temperature of the first pass is 120-200°C. In the 2nd to 5th passes, an emulsion with a mass percentage concentration of 5-8% and a temperature of 50-70°C is used to lubricate and cool the strip in a "medium temperature mode" so that the strip outlet temperature is 70-120°C.
[0050] In the primary cold rolling step, a working roll with high roughness is used for rolling. In some more specific embodiments, the working roll with high roughness has a roughness of 1.0-2.5 μm.
[0051] Figure 2 A schematic diagram of the emulsion injection control of the first pass in a cold rolling step in some embodiments of the cold rolling pressure processing method described in the present invention is shown.
[0052] like Figure 2 As shown, in the "high temperature mode", the strip cooling nozzle 1 at the rolling pass entrance, the strip cooling nozzle 4 at the rolling pass exit, and the roll gap lubrication cooling nozzle 3 at the rolling pass exit are all closed, and the roll gap lubrication cooling nozzle 2 at the rolling pass entrance is opened.
[0053] Figure 3 A schematic diagram showing emulsion injection control for 2-5 passes in a cold rolling step in some embodiments of the cold rolling pressure processing method of the present invention is shown.
[0054] like Figure 3 As shown, in the "medium temperature mode", the strip cooling nozzle 1 at the rolling pass entrance and the strip cooling nozzle 4 at the rolling pass exit are controlled to be closed, and the roll gap lubrication cooling nozzle 3 at the rolling pass exit and the roll gap lubrication cooling nozzle 2 at the rolling pass entrance are controlled to be opened.
[0055] 500: Intermediate annealing: A sleeve is set on the annealing unit exit coiler in the intermediate annealing step.
[0056] 600: Secondary cold rolling: a single-stand rolling mill is used for reciprocating rolling, through an even number of passes, in some embodiments, 2 or 4 passes, to a finished product thickness of 0.15-0.3 mm, wherein the reduction rate of each pass is controlled to be 30%-45%, and the entrance tension of each pass is controlled to be 90-180 N / mm 2 The exit tension of each rolling pass is controlled at 160-260N / mm 2During the rolling process, the strip is lubricated and cooled in a "low temperature mode" using an emulsion with a mass percentage concentration of 3-8% and a temperature of 50-70°C, so that the strip outlet temperature is 50-75°C.
[0057] Figure 4 A schematic diagram of emulsion injection control in the secondary cold rolling step of the cold rolling pressure processing method according to some embodiments of the present invention is shown.
[0058] like Figure 4 As shown, in the "low temperature mode", the strip cooling nozzles at the rolling pass entrance, the strip cooling nozzles at the rolling pass exit, the roll gap lubrication cooling nozzles at the rolling pass exit and the roll gap lubrication cooling nozzles at the rolling pass entrance are all turned on.
[0059] In the secondary cold rolling step, a low-roughness work roll is used for rolling. In some more specific embodiments, the roughness of the low-roughness work roll is 0.1-0.5 μm.
[0060] Table 1 lists the product parameters of the high silicon and high aluminum non-oriented silicon steel used in Examples 1-6 of the present invention.
[0061] Table 1.
[0062]
[0063] Table 2-1 and Table 2-2 list the specific process parameters used in each step of Examples 1-6 of the present invention.
[0064] Table 2-1.
[0065]
[0066]
[0067]
[0068] Table 2-2.
[0069]
[0070]
[0071] The non-oriented silicon steel product prepared by the present invention has high rolling stability, the breaking rate of the rolling strip during the first cold rolling is below 1.3%, and the breaking rate of the rolling strip during the second cold rolling is controlled below 1%.
[0072] The non-oriented silicon steel product prepared by the present invention can achieve a 7I plate shape qualification rate of more than 97% in the first cold rolling, a 7I plate shape qualification rate of more than 99% in the second cold rolling, and a strip surface roughness of less than 0.2um.
[0073] It should be noted that the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0074] It should also be noted that the above-listed embodiments are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therewith can be directly derived or easily associated with the contents disclosed by those skilled in the art from the present invention, and all should belong to the protection scope of the present invention.
Claims
1. A cold rolling pressure processing method for non-oriented silicon steel products, comprising a primary cold rolling step and a secondary cold rolling step, characterized in that: In the first cold rolling step: a single-stand rolling mill is used for reciprocating rolling, and a first-rolled intermediate strip is formed through 3-5 passes, wherein the rolling reduction rate of each pass is controlled between 17-38%, and the entrance tension of each pass is controlled between 50-150N / mm 2 The exit tension of each rolling pass is controlled at 120-220N / mm 2 ; And during the rolling process, the strip is lubricated and cooled with emulsion so that the strip outlet temperature of the first pass is 120-200℃, and the strip outlet temperature of the 2nd to 5th pass is 70-120℃; In the secondary cold rolling step: a single-stand rolling mill is used for reciprocating rolling, and the product thickness is reached through an even number of passes, wherein the reduction rate of each pass is controlled to be 30%-45%, and the entrance tension of each pass is controlled to be 90-180N / mm 2 The exit tension of each rolling pass is controlled at 160-260N / mm 2 ; And during the rolling process, emulsion is used to lubricate and cool the strip so that the strip outlet temperature is 50-75℃.
2. The cold rolling pressure processing method according to claim 1, characterized in that: In the first cold rolling step, the emulsion is used to lubricate and cool the strip, specifically including: In the first pass, the strip cooling nozzles at the rolling pass entrance, the strip cooling nozzles at the rolling pass exit, and the roll gap lubrication cooling nozzles at the rolling pass exit are all closed, and the roll gap lubrication cooling nozzles at the rolling pass entrance are opened; In the 2nd to 5th passes, the strip cooling nozzles at the rolling pass entrance and the strip cooling nozzles at the rolling pass exit are controlled to be closed, and the roll gap lubrication cooling nozzles at the rolling pass exit and the roll gap lubrication cooling nozzles at the rolling pass entrance are controlled to be opened.
3. The cold rolling pressure processing method according to claim 1, characterized in that: In the secondary cold rolling step, the emulsion is used to lubricate and cool the strip, specifically including: controlling the strip cooling nozzle at the rolling pass entrance, the strip cooling nozzle at the rolling pass exit, the roll gap lubrication cooling nozzle at the rolling pass exit and the roll gap lubrication cooling nozzle at the rolling pass entrance to be open.
4. The cold rolling pressure processing method according to claim 1, characterized in that: In the primary cold rolling step, rolling is performed using work rolls having a roughness of 1.0-2.5 μm.
5. The cold rolling pressure processing method according to claim 1, characterized in that: In the secondary cold rolling step, rolling is performed using work rolls having a roughness of 0.1-0.5 μm.
6. The cold rolling pressure processing method according to claim 1, characterized in that: In the primary cold rolling step, the normalized pickled strip with a thickness of 1.5-2.4 mm is rolled into a primary rolled intermediate strip with a thickness of 0.5-0.7 mm.
7. The cold rolling pressure processing method according to claim 1, characterized in that: In the first cold rolling step, the temperature of the emulsion is 50-70° C.; and / or the mass percent concentration of the emulsion is 5-8%.
8. The cold rolling pressure processing method according to claim 1, characterized in that: In the first cold rolling step, the temperature of the emulsion is 50-70° C.; and / or the mass percent concentration of the emulsion is 3-8%.
9. The cold rolling pressure processing method according to claim 1, characterized in that: In the secondary cold rolling step, the rolling passes are 2 or 4.
10. The cold rolling pressure processing method according to claim 1, characterized in that: Before the primary cold rolling step, a leader strip with a length of 5-20 m is welded at the head and tail of the strip.
11. The cold rolling pressure processing method according to claim 1, characterized in that: There is an intermediate annealing step between the primary cold rolling step and the secondary cold rolling step, and a sleeve is provided on the exit coiler of the annealing unit in the intermediate annealing step.
12. The cold rolling pressure processing method according to claim 1, characterized in that: The invention is used for non-oriented silicon steel products with Si+Al mass percentage of 3.5-5.0%.
13. The cold rolling pressure processing method according to claim 1, characterized in that: The finished product has a thickness of 0.15-0.3 mm.
14. The cold rolling pressure processing method according to any one of claims 1 to 13, characterized in that: Prior to the primary cold rolling step, the normalized pickled strip is heated.
15. The cold rolling pressure processing method according to claim 14, characterized in that: The heating temperature is 100-150°C.
Citation Information
Patent Citations
Cold rolling method for preventing high-silicon strip steel from being broken
CN102476131A
Cold rolling method for high-silicon steel with Si content equal to or higher than 2.5%
CN108213077A
High-silicon non-oriented electrical steel and production method thereof
CN112080695A
Cold rolling method of ultra-thin and ultra-low iron loss oriented silicon steel
CN115837403A
Production of nonoriented silicon steel sheet reduced in iron loss
JP1994293922A