Pipe-pipe butt welding process and device with corrosion-resistant alloy layers coated in pipe ends
By employing a pipe-to-pipe butt welding process with an inner corrosion-resistant alloy layer on the pipe end, and utilizing a magnetic molten iron device and stainless steel argon-free self-shielded welding wire, the problem of brittle carbide structures such as martensite in the butt weld joint of the pipe-to-pipe butt weld with an inner corrosion-resistant alloy layer on the pipe end was solved, thereby improving joint performance and extending pipeline life.
Patent Information
- Application Number
- CN202411056654.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing technology, pipe butt welds with corrosion-resistant alloy layers lining the pipe ends are prone to forming brittle carbide structures such as martensite during the welding process, resulting in poor mechanical and corrosion properties of the joint, which affects the safe operation and service life of the pipeline.
A pipe-to-pipe butt welding process with an inner corrosion-resistant alloy layer at the pipe end is adopted, including step 1: pipe end cleaning, step 2: weld joint assembly and tack welding, step 3: setting up a magnetic molten iron gathering device, step 4: root pass argon arc welding, step 5: fill pass shielded metal arc welding, and step 6: cover pass shielded metal arc welding. The magnetic molten iron gathering device is used to gather the molten iron, and stainless steel argon-free self-shielded welding wire and optimized welding current and electrode manipulation are used to avoid nickel-based alloy transition layers.
It effectively reduces the formation of martensite and other carbide structures, improves the mechanical and corrosion properties of the joint, extends the service life of the pipeline, and has a simple process and low cost, making it suitable for pipe connections of different diameters and wall thicknesses.
Smart Images

Figure CN118905395A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding, relates to pipe-to-pipe butt welding, and specifically relates to a pipe-to-pipe butt welding process and a device for pipe ends covered with a corrosion-resistant alloy layer. Background Art
[0002] The produced fluid medium of the oilfield surface system is complex, with high mineralization content and CO2 and H2S in the highly acidic environment, which poses great difficulties for oil and gas transportation. The low-carbon pipeline steel used for traditional transportation is prone to medium leakage accidents due to its poor corrosion resistance. If the entire pipe is made of stainless steel, nickel-based alloy or the inner wall of the entire pipe is made of corrosion-resistant alloy as a transportation pipeline, the cost is relatively high. In recent years, oil and gas field enterprises have adopted factory-prefabricated anti-corrosion technology of coating epoxy powder inside the pipe body + covering the pipe end with a corrosion-resistant alloy layer, which has a lower cost. Generally, the corrosion-resistant alloy layer inside the pipe end is stainless steel or nickel-based alloy, and the pipe substrate is carbon steel. However, during the on-site pipe-to-pipe butt welding process, the pipeline steel with a corrosion-resistant alloy layer inside the pipe end is easily affected by the physical and chemical properties of the two materials, and brittle carbide structures such as martensite are easily formed at the interface of the two materials and the weld of the weld joint, and the mechanical properties and corrosion properties of the joint are poor, which poses a huge threat to the safe operation of the pipeline.
[0003] Usually, the pipe-to-pipe butt welding with the corrosion-resistant alloy layer inside the pipe end attempts to solve this problem by using a nickel-based alloy transition method at the interface between the two materials, but carbide structures such as martensite will still be formed. This is because the base layer is stainless steel and the transition layer is a nickel-based alloy. When a carbon steel electrode with the same composition as the pipe matrix is used to weld the nickel-based alloy, the nickel-based alloy melts, and the Cr in the nickel-based alloy enters the carbon steel to form carbide structures such as martensite, resulting in poor mechanical properties and corrosion properties of the welded joint and a short service life of the pipeline. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a pipe-to-pipe butt welding process and device with a corrosion-resistant alloy layer coated on the pipe end, so as to solve the technical problem that the defect of carbide structure formed in the welding joint of the pipe-to-pipe butt welding process in the prior art needs to be further reduced.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0006] A pipe-to-pipe butt welding process with a pipe end coated with a corrosion-resistant alloy layer, the process comprising the following steps:
[0007] Step 1: Clean the pipe end:
[0008] Step 2: Weld joint assembly and spot fixing:
[0009] Step 3: arranging magnetic molten iron devices at both ends of the pipes:
[0010] After the weld joint pairing and spot fixing in step 2, magnetic molten iron gathering devices are installed at both ends of the groove. The distance between the magnetic molten iron gathering devices and the groove of the pipe end is 15 to 20 mm. A pair of magnetic molten iron gathering devices are symmetrically arranged at the pipe ends on both sides, and the S pole is close to the groove side.
[0011] Step 4: Base layer welding:
[0012] The base layer is welded in two half-circles, left and right. The base layer is welded by argon arc welding. The welding wire of argon arc welding adopts stainless steel argon-free self-shielded welding wire with the chemical composition consistent with the corrosion-resistant alloy coating. After the base layer is welded, the thickness of the weld layer is 1.4mm~2mm.
[0013] Step 5: Filling layer welding:
[0014] The filling layer is welded by arc welding with a welding current of 65 to 80A.
[0015] After the filling layer is welded, the weld surface should be slightly lower than the edge of the upper surface of the groove by 0.5 to 1 mm, keeping the edge of the upper surface of the groove in its original state.
[0016] After the filling layer is welded, the microhardness of the filling layer in the weld cross section should be lower than 350Hv.
[0017] Step 6: Cover layer welding:
[0018] The cover layer is welded by arc welding with a welding current of 70 to 85A.
[0019] The present invention also has the following technical features:
[0020] In step three, the magnetic molten iron gathering device includes a magnet attractor, which includes an austenitic stainless steel shell, on which a bar magnet seat mounting hole is provided along the longitudinal direction; chromium-zirconium-copper magnetic isolation blocks are respectively provided along the longitudinal direction on the austenitic stainless steel shell on both sides of the horizontal outside the bar magnet seat mounting hole, a bar magnet seat is installed in the bar magnet seat mounting hole, a bar magnet and a knob switch are provided on the bar magnet seat, the knob switch drives the bar magnet on the bar magnet seat to rotate together in the bar magnet seat mounting hole, and when the end of the bar magnet is flush with the chromium-zirconium-copper magnetic isolation block, the chromium-zirconium-copper magnetic isolation block can isolate the bar magnet from magnetism.
[0021] A suction opening is arranged longitudinally on the lateral inner side of the austenitic stainless steel shell, the opening of the suction opening is laterally away from the bar magnet seat mounting hole, the bottom of the suction opening is laterally close to the bar magnet seat mounting hole, and a second V-shaped groove arranged longitudinally is opened at the bottom of the suction opening, and two groove surfaces of the second V-shaped groove are arranged tangent to the suction opening.
[0022] A permanent magnet is arranged on one side of the austenitic stainless steel shell near the groove. The structure of the permanent magnet is a semicircular ring structure. The inner diameter of the permanent magnet, the inner diameter of the suction opening and the radius of the pipe to be butt-welded are the same.
[0023] A first magnetic isolation sheet made of austenitic stainless steel is arranged between the permanent magnet and the magnetic attractor.
[0024] The vertical upper part and lower part of the semicircular opening of the magnet attractor and the permanent magnet are respectively provided with austenitic stainless steel second magnetic isolation sheets.
[0025] Preferably, the pipe fittings to be butt-welded have a pipe diameter of 60 to 114 mm, a pipe wall thickness of 5 to 6 mm, and a corrosion-resistant alloy layer thickness of 1.5 to 2 mm.
[0026] The specific process of step one is: use a straight-shank angle grinder equipped with a handle flap wheel cylindrical grinding head to grind the outer wall of the pipe end with a groove within 20 to 30 mm to expose the metallic luster, and then use a straight-shank angle grinder equipped with a handle brown corundum conical grinding wheel grinding head to clean the inner wall of the pipe end within 15 to 20 mm.
[0027] The specific process of step 2 is: place the two pipe ends covered with the corrosion-resistant alloy layer in the first V-shaped groove prepared in advance, and assemble them with a gap of 3.0 to 4.5 mm. After the assembly is completed, the two pipe ends are spot-fixed by argon arc welding in a free state, and the spot-fixed length is 8 to 10 mm.
[0028] In step 2, the first V-shaped groove is a pairing device formed by welding two identical pipes together tangentially, with a length of 500 to 600 mm. The diameter of a single pipe of the first V-shaped groove is 1.5 to 2 times the diameter of the pipe to be butt-welded.
[0029] In step 2, the argon arc welding machine is a plug-in and rechargeable dual-purpose welding machine that integrates electrode arc welding and argon arc welding.
[0030] The method further includes:
[0031] Step 7, post-weld treatment:
[0032] Step 8: Appearance inspection:
[0033] Step 9, Rework:
[0034] The welding process from step 1 to step 7 is used to perform repair welding of the pipe fitting.
[0035] The present invention also protects a magnetic molten iron gathering device, which is the magnetic molten iron gathering device described in the above step three.
[0036] Compared with the prior art, the present invention has the following technical effects:
[0037] (I) The process of the present invention is simple, low-cost, and high-efficiency. It is not easy to form carbide structures such as martensite. The mechanical properties and corrosion resistance of the joint are significantly improved, effectively extending the service life of the pipeline.
[0038] (II) The process of the present invention is suitable for pipes with a diameter of 60 to 114 mm and a wall thickness of (5 to 6) + (1.5 to 2 corrosion-resistant alloy layers) mm, and can achieve good connection.
[0039] (III) After the pipes are assembled and spot-fixed in the process of the present invention, magnetic molten iron gathering devices are installed on both sides of the pipe end grooves. This device has a gathering effect on the molten iron when the carbon steel filling layer is welded, and the molten iron dissipates heat slowly.
[0040] (IV) In the process of the present invention, stainless steel argon-free self-shielded welding wire is used for argon arc welding for base coating, and electrode arc welding for filling and covering is used for welding, thereby omitting the nickel-based alloy transition layer between the base coating and the filling layer in the traditional pipe-to-pipe butt welding with a corrosion-resistant alloy layer at the pipe end, thereby ensuring a thicker weld layer thickness of the filling layer and making the weld cooling rate low.
[0041] (V) In the process of the present invention, the preferred welding current and the appropriate welding rod feeding method are selected for base welding, filling welding and cap welding.
[0042] (VI) The process of the present invention eliminates carbide structures such as martensite in the welded joint, significantly improves the joint performance, the tensile fracture is located in the parent material area, and the intergranular corrosion is intact. The welding process is simple, efficient and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic diagram of the structure of the magnetic molten iron device in the present invention.
[0044] Figure 2 for Figure 1 Schematic diagram of the B-direction structure.
[0045] Figure 3 It is a schematic diagram of the first V-shaped groove of the weld joint group of the present invention.
[0046] Figure 4 It is a schematic diagram of the pipe-to-pipe butt welding structure of the present invention in which the pipe ends are covered with a corrosion-resistant alloy layer.
[0047] Figure 5 This is the macroscopic morphology of the cross section of the joint after welding in Example 3.
[0048] Figure 6 Schematic diagram of the interface between the primer and the filling layer in Example 3.
[0049] Figure 7 This is a schematic diagram of the filling layer in Example 3.
[0050] Figure 8 This is the microhardness diagram of the cross section of the joint in Example 3.
[0051] Fig. 9 This is the mutual diffusion diagram of C element at the interface between the base layer and the filling layer in Example 3.
[0052] Fig.10 This is the mutual diffusion diagram of Cr element at the interface between the base layer and the filling layer in Example 3.
[0053] Fig.11 This is a diagram of the tensile fracture specimen in Example 3.
[0054] Fig.12 These are the face bending and back bending specimens in Example 3.
[0055] Fig.13 This is the macroscopic morphology of the cross section of the welded joint in Comparative Example 1.
[0056] Fig.14 Schematic diagram of the interface between the transition layer and the base layer in Comparative Example 1.
[0057] Fig.15 This is a schematic diagram of the filling layer in Comparative Example 1.
[0058] Fig.16 This is the microhardness diagram of the cross section of the joint in Comparative Example 1.
[0059] Fig.17 This is the mutual diffusion diagram of C element at the interface between the transition layer and the filling layer in comparative example 1.
[0060] Fig.18 This is the mutual diffusion diagram of Cr element at the interface between the transition layer and the filling layer in comparative example 1.
[0061] Fig.19 This is the tensile fracture specimen diagram in Comparative Example 1.
[0062] Fig. 20 These are the face bending and back bending specimens in Comparative Example 1.
[0063] Fig.21 This is the tensile fracture diagram in Comparative Example 1.
[0064] Fig. 22 This is the macroscopic morphology of the cross section of the welded joint in Comparative Example 2.
[0065] Fig.23 This is a schematic diagram of the filling layer in Comparative Example 2.
[0066] Fig.24 This is the tensile fracture specimen diagram in Comparative Example 2.
[0067] Fig.25These are the face bending and back bending specimens in Comparative Example 2.
[0068] Fig.26 This is the macroscopic morphology of the cross section of the welded joint in Comparative Example 3.
[0069] Fig. 27 Schematic diagram of the interface between the base material and the filling layer in Comparative Example 3.
[0070] Fig.28 This is the tensile fracture specimen diagram in Comparative Example 3.
[0071] Fig.29 These are the face bending and back bending specimens in Comparative Example 3.
[0072] Fig.30 This is the macroscopic morphology of the cross section of the welded joint in Comparative Example 4.
[0073] Fig.31 This is a schematic diagram of the interface between the base material and the filling layer and the filling layer in Comparative Example 4.
[0074] Fig.32 This is a schematic diagram of the interface of the cover layer in Comparative Example 4.
[0075] Fig.33 This is the tensile fracture specimen diagram in Comparative Example 4.
[0076] Fig.34 These are the face bending and back bending specimens in Comparative Example 4.
[0077] Fig.35 This is the macroscopic morphology of the cross section of the welded joint in Example 4.
[0078] Fig.36 Schematic diagram of the interface between the base material and the filling layer and the filling layer in Example 4.
[0079] Fig.37 This is a diagram of the tensile fracture specimen in Example 4.
[0080] Fig.38 These are the face bending and back bending specimens in Example 4.
[0081] Fig.39 This is the intergranular corrosion sample diagram in Example 4.
[0082] Fig.40 This is the filling layer fusion line and filling layer in Comparative Example 5.
[0083] Fig.41 This is the tensile fracture specimen diagram in Comparative Example 5.
[0084] Fig.42 These are the face bending and back bending specimens in Comparative Example 5.
[0085] Fig.43 This is the intergranular corrosion sample diagram in Comparative Example 5.
[0086] The meanings of the numbers in the figure are: 1-magnet attractor, 2-austenitic stainless steel shell, 3-bar magnet seat mounting hole, 4-chromium zirconium copper magnetic isolation block, 5-bar magnet seat, 6-attraction port, 7-second V-shaped groove, 8-bar magnet, 9-permanent magnet, 10-austenitic stainless steel first magnetic isolation plate, 11-austenitic stainless steel second magnetic isolation plate, 12-knob switch, 13-first V-shaped groove, 14-pipe fittings to be butt-welded, 15-base pipe, 16-corrosion-resistant alloy coating, 17-base layer, 18-filling layer, 19-covering layer.
[0087] The specific contents of the present invention are further explained in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0088] It should be noted that, unless otherwise specified, all raw materials, reagents and equipment in the present invention are raw materials, reagents and equipment known in the prior art and can be obtained from commercial channels.
[0089] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0090] Embodiment 1:
[0091] This embodiment provides a magnetic molten iron device, such as Figure 1 and Figure 2 As shown, it includes a magnet attractor 1, which includes an austenitic stainless steel shell 2, and a bar magnet seat mounting hole 3 is opened on the austenitic stainless steel shell 2 along the longitudinal direction; chromium-zirconium-copper magnetic isolation blocks 4 are respectively arranged on the austenitic stainless steel shell 2 on both sides of the bar magnet seat mounting hole 3 along the longitudinal direction, a bar magnet seat 5 is installed in the bar magnet seat mounting hole 3, and a bar magnet 8 and a knob switch 12 are arranged on the bar magnet seat 5. The knob switch 12 drives the bar magnet 8 on the bar magnet seat 5 to rotate together in the bar magnet seat mounting hole 3. When the end of the bar magnet 8 is flush with the chromium-zirconium-copper magnetic isolation block 4, the chromium-zirconium-copper magnetic isolation block 4 can isolate the bar magnet 8;
[0092] A suction opening 6 is arranged longitudinally on the lateral inner side of the austenitic stainless steel shell 2, the opening of the suction opening 6 is laterally away from the bar magnet seat mounting hole 3, the bottom of the suction opening 6 is laterally close to the bar magnet seat mounting hole 3, and a second V-shaped groove 7 arranged longitudinally is opened at the bottom of the suction opening 6, and two groove surfaces of the second V-shaped groove 7 are tangent to the suction opening 6;
[0093] A permanent magnet 9 is arranged on one side of the austenitic stainless steel shell 2 near the groove. The structure of the permanent magnet 9 is a semicircular ring structure. The inner diameter of the permanent magnet 9, the inner diameter of the suction opening 6 and the radius of the pipe 14 to be butt-welded are the same.
[0094] An austenitic stainless steel first magnetic isolation sheet 10 is provided between the permanent magnet 9 and the magnetic attractor 1 ; the purpose of providing the first magnetic isolation sheet 10 is to prevent the magnetic fields generated between the magnetic attractor 1 and the permanent magnet 9 from interfering with each other.
[0095] The upper and lower parts of the semicircular opening of the magnet attractor 1 and the permanent magnet 9 are respectively provided with austenitic stainless steel second magnetic shielding plates 11. The purpose of providing the second magnetic shielding plates 11 is to prevent the magnetic fields generated between the symmetrically arranged magnetic iron molten devices of the pipes 14 to be butt-welded from interfering with each other.
[0096] In this embodiment, the purpose of the magnet attractor 1 is to conveniently fix the magnetic iron collecting device on the pipe end of the pipe 14 to be butt-welded, and to facilitate removal when not in use. The working principle of the magnet attractor 1 is to use the principle that the magnetic field strength of the upper and lower parts and the left and right ends of the bar magnet 8 is different, and rely on the rotating magnetic field to achieve magnetic adsorption. When the knob switch 12 rotates 90°, so that the upper and lower parts of the bar magnet 8 are aligned with the pipe (magnetic conductor) enclosed by the second V-shaped groove 7 and the suction port 6, due to the large magnetic field strength and large magnetic force, it can be adsorbed on the pipe 14 to be butt-welded. On the contrary, when the left and right ends of the bar magnet 8 are aligned with the pipe (magnetic conductor) enclosed by the second V-shaped groove 7 and the suction port 6, due to the small magnetic field strength and small magnetic force, and under the action of the chromium-zirconium-copper magnetic isolation block 4, the magnet attractor 1 does not attract the pipe 14 to be butt-welded.
[0097] Embodiment 2:
[0098] This embodiment provides a pipe-to-pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. Before performing the pipe-to-pipe butt welding process of the present invention, the following steps need to be performed in a factory:
[0099] First, the pipe end is covered with a corrosion-resistant alloy layer, and the microhardness value of the corrosion-resistant alloy layer should be lower than 250Hv; second, the pipe end is grooved: the two pipe ends are processed into a V-shaped groove by a groove machine, and the groove angle is 50°±5°.
[0100] The process includes the following steps:
[0101] Step 1: Clean the pipe end:
[0102] Use a straight-shank angle grinder equipped with a handle flap wheel cylindrical grinding head to grind the outer wall of the pipe end with a groove within 20 to 30 mm to reveal the metallic luster. Then use a straight-shank angle grinder equipped with a handle brown corundum conical grinding wheel grinding head to clean the inner wall of the pipe end within 15 to 20 mm.
[0103] Step 2: Weld joint assembly and spot fixing:
[0104] like Figure 3 As shown, the two pipe ends covered with the corrosion-resistant alloy layer are placed in the first V-shaped groove 13 prepared in advance for pairing, and the pairing gap is 3.0-4.5 mm. After the pairing is completed, the two pipe ends are in a free state and spot-fixed by argon arc welding. The welding materials used for spot-fixing are the same as those for normal base welding. Spot-fixing is performed at the 10 o'clock and 2 o'clock positions, and the spot-fixing length is 8-10 mm.
[0105] In step 2, the first V-shaped groove 13 is a pairing device formed by welding two identical pipes together at the outer wall generatrix, with a length of 500-600 mm, and a single pipe diameter of the first V-shaped groove 13 is 1.5-2 times the diameter of the pipe 14 to be butt-welded. The pairing is performed by the first V-shaped groove 13, which is simple, low-cost and easy to use.
[0106] In step 2, the argon arc welding machine is a plug-in and rechargeable dual-purpose welding machine that integrates arc welding and argon arc welding, has a built-in lithium battery, carries four 300mm diameter rubber wheels, has a welding primary voltage of 220V, and a welding current range of 10A to 200A. The welding machine is easy to use and plays a great role in places without electricity, and is suitable for field construction.
[0107] Step 3: arranging magnetic molten iron devices at both ends of the pipes:
[0108] After the weld joint pairing and spot fixing in step 2, magnetic molten iron gathering devices are installed at both ends of the groove. The distance between the magnetic molten iron gathering devices and the groove of the pipe end is 15 to 20 mm. Two pairs of magnetic molten iron gathering devices are symmetrically arranged on both sides of the pipe end (front and back or left and right), and the S pole is close to the groove side.
[0109] The magnetic molten iron gathering device adopts the magnetic molten iron gathering device given in Example 1.
[0110] In this embodiment, the two S poles in the magnetic molten iron gathering device are opposite, which results in the same direction of the magnetic field generated at both ends of the groove, so that the magnetic field energy increases, and the system tends to reduce the energy. Therefore, the magnetic molten iron gathering device has a gathering effect on the molten iron, achieving the effect of slow heat dissipation of the molten iron.
[0111] Step 4: Base layer welding:
[0112] like Figure 4 As shown, the base layer is welded in two half-circles, left and right. The base layer is welded by argon arc welding. The welding wire of argon arc welding adopts stainless steel argon-free self-shielded welding wire with the chemical composition consistent with the corrosion-resistant alloy coating. After the base layer is welded, the thickness of the weld layer is 1.4mm~2mm.
[0113] Specifically in this step, the arc is struck on the groove slope, welding starts from the 6 o'clock overhead welding position, and the arc is closed at the 12 o'clock flat welding position.
[0114] The welding wire model for argon arc welding is TGF316 stainless steel argon-free self-shielded welding wire, whose chemical composition is consistent with the corrosion-resistant alloy coating, with a diameter of 2.5mm and a welding current of 105A to 125A. The microhardness of the base layer after welding is close to that of the corrosion-resistant alloy coating and is lower than 200Hv, otherwise cracks are likely to occur in the back bend.
[0115] During welding, the welding gun swings in a crescent shape and forms a uniform melt hole with a diameter of 2mm to 3mm to ensure full penetration and good formation of the back of the weld. The welding gun swings to both sides of the groove and stays for about 0.3s to 0.5s to allow the root of the groove to be fully fused. When encountering a weld joint, use an angle grinder to grind the joint into a slope to ensure full fusion at the joint and prevent defects such as incomplete penetration.
[0116] The thickness of the welding layer is 1.4mm to 2mm, excluding the inner convex thickness, which is strictly prohibited to be greater than 2mm. The upper limit of the base thickness is stipulated to prevent the thickness of the next filling layer from being thinned.
[0117] Step 5: Filling layer welding:
[0118] The filling layer is welded by arc welding with a welding current of 65 to 80A.
[0119] After the filling layer is welded, the weld surface should be slightly lower than the edge of the upper surface of the groove by 0.5 to 1 mm, keeping the edge of the upper surface of the groove in its original state.
[0120] After the filling layer is welded, the microhardness of the filling layer in the weld cross section should be lower than 350Hv.
[0121] Specifically in this embodiment, before welding the filling layer, a 60-mesh brown corundum flap wheel angle grinder is used to clean the slag and spatter on the surface of the base layer weld and the weld roots on both sides, and welding can be carried out after cleaning.
[0122] The welding is the same as the base layer, and is also divided into two half-cycles, but the welding starts from the overhead welding position at 6:20 and ends at the flat welding position at 12:20. The welding rod is used for arc welding. The welding rod model is E4315, with a diameter of 2.5mm. The welding rod should be dried strictly in accordance with relevant standards. The welding current is 65-80A. The arc should be struck on the groove slope or the base layer. If the arc is struck on the base layer, it must be struck on the upper part of the starting welding position. After the arc is ignited, the arc is pulled to the starting welding position.
[0123] During welding, the electrode should be swung in a zigzag shape. It is strictly forbidden to use a crescent shape. The electrode should be swung to both sides of the weld for about 1s to 2s to ensure good fusion on both sides of the groove and prevent the occurrence of unfused. The purpose of using a zigzag shape instead of a crescent shape is to avoid bringing the base or cladding stainless steel structure into the carbon steel to form carbides such as martensite.
[0124] After the filling layer is welded, the weld surface should be slightly lower than the upper edge of the groove by 0.5 to 1 mm, keeping the upper edge of the groove in its original state. There are two reasons for such a process design: first, it lays a benchmark for the neat and straight appearance of the lower cover weld; second, it ensures that the thickness of the filling layer is 3.5 to 4.5 mm, avoiding the formation of carbide structures such as martensite due to the thin thickness of the filling layer and the fast cooling rate.
[0125] In addition, after filling welding, the microhardness of the filling layer in the weld cross section should be lower than 350Hv. If it reaches above 400Hv, it means that brittle hardening structures such as martensite have been generated.
[0126] Step 6: Cover layer welding:
[0127] The cover layer is welded by arc welding with a welding current of 70 to 85A.
[0128] Specifically, before the cap welding, the slag and spatter on the surface of the filler layer weld are cleaned with a 60-mesh brown corundum flap angle grinder. After cleaning, welding is started when the interlayer temperature is less than 200°C. The welding rod is used for arc welding. The welding rod model is E4315, the welding rod diameter is 2.5mm, the welding rod drying is the same as the base layer, the welding current is 70-85A, and the arc is struck on the filler layer. The arc striking operation is the same as the base layer. Start welding from the 6 o'clock overhead welding position and end the arc at the 12 o'clock flat welding position.
[0129] During welding, zigzag or reverse crescent swing continuous welding is used. When the electrode swings to the edges of both sides of the groove, the arc is depressed and stays on both sides for about 1.5 to 2.0 seconds. When capping, the upper surface of the base material on both sides of the groove should be covered by 1 to 2 mm to prevent undercut and unfused welds on both sides of the weld after welding. The weld excess height should be controlled between 1 and 2 mm. The arc pit surface should be filled when welding to prevent defects such as arc pits and cracks.
[0130] Step 7, post-weld treatment:
[0131] Specifically, after welding, a slag hammer is used to clean the slag on the surface of the cover layer, and a rubber hammer is used to knock on both sides of the weld to make the slag on the inner surface of the base layer self-shielding welding wire fall off. Then, high-pressure gas is used to purge the inside of the pipeline. This process solves the problem of non-welding defects in the weld seam detected by X-ray film after welding.
[0132] Step 8: Appearance inspection:
[0133] Specifically, the weld surface must not have cracks, lack of fusion, pores, slag inclusions, arcing marks, weld bumps, pits and other defects, and the appearance must be uniform. If there is spatter near the weld, use an angle grinder to clean it up, and the weld must not be damaged during cleaning.
[0134] Step 9, Rework:
[0135] The welding process from step 1 to step 7 is used to perform repair welding of the pipe fitting.
[0136] Specifically in this step, all cracks, pores and other defective welds, except for arc crater cracks, should be cut or polished, including the heat-affected zone. Oxyacetylene cutting or plasma cutting is prohibited during cutting. The same weld position shall not be repaired more than twice, and the root weld is only allowed to be repaired once. Welds that are still unqualified after two repairs need to have the entire weld including the heat-affected zone removed, and the repaired welds should be re-tested using the original test method.
[0137] Embodiment 3:
[0138] This embodiment provides a pipe-to-pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end based on Embodiment 2. In this embodiment, the pipe end having the corrosion-resistant alloy layer coated on the pipe end has a diameter of 60 mm, a wall thickness of (5+2) mm, a groove angle of 52°, a pair gap of 4 mm, and a microhardness of the inner corrosion-resistant alloy layer less than 250 Hv (microhardness of the base layer 4 mm away from the center of the weld).
[0139] Before welding, a magnetic hot metal device was installed. The welding process and parameters are shown in Table 1. The macroscopic morphology of the cross section of the joint after welding is as follows: Figure 5 As shown; no martensite formation was observed at the interface between the base layer and the filling layer, as well as in the filling layer ( Figure 6 and Figure 7 The microhardness of the filling layer and the cover layer is lower than 350Hv ( Figure 8 The mutual diffusion of C and Cr elements at the interface between the base layer and the filling layer is not obvious ( Fig. 9 and Fig.10 After welding with this process and parameters, tensile and bending tests were carried out according to NB / T47014-2011 standard. The tensile fracture was located in the base material, and the elongation was high ( Fig.11 ), the face and back curves are intact ( Fig.12 ).
[0140] Table 1 Welding process and parameters
[0141]
[0142] Comparative Example 1:
[0143] This comparative example provides a pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. In this comparative example, the pipe with the corrosion-resistant alloy layer coated on the pipe end has a diameter of 60 mm, a wall thickness of (5+2) mm, a groove angle of 52°, a pair gap of 4 mm, and a microhardness of the inner corrosion-resistant alloy layer less than 250 Hv (the microhardness of the base layer 4 mm away from the center of the weld).
[0144] The difference from Example 3 is that a transition layer is added to reduce the thickness of the filling layer. The welding process and parameters are shown in Table 2. The macroscopic morphology of the cross section of the welded joint is as follows: Fig.13 As shown; martensite structure can be seen in the filling layer, transition layer and filling layer ( Fig.14 and Fig.15 ); the hardness of the filling layer reaches 450Hv ( Fig.16 ), indicating the formation of martensite. The mutual diffusion of C and Cr elements at the interface between the transition layer and the filling layer is obvious ( Fig.17 and Fig.18 After welding with this process and parameters, tensile and bending tests were carried out according to NB / T47014-2011 standard. The tensile fracture was located at the weld and the elongation was low ( Fig.19 ), both the back bend and the face bend are broken from the weld ( Fig. 20 ), the left and right sides of the tensile fracture show ductile and brittle fractures respectively ( Fig.21 ), analysis shows that the left side is the transition layer and the right side is the filling layer.
[0145] Table 2 Welding process and parameters
[0146]
[0147] Comparative Example 2:
[0148] This comparative example provides a pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. In this comparative example, the pipe with the corrosion-resistant alloy layer coated on the pipe end has a diameter of 60 mm, a wall thickness of (5+2) mm, a groove angle of 52°, and a pair gap of 4 mm.
[0149] The difference from Example 3 is that the thickness of the filling layer is reduced. Fig. 22 As shown; martensite formation can be seen in the filling layer ( Fig.23 );Joint fracture is in the center of weld ( Fig.24 After welding with this process and parameters, according to the NB / T47014-2011 standard bending test, cracks appeared in both the face bend and the back bend ( Fig.25 ).
[0150] Comparative Example 3:
[0151] This comparative example provides a pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. In this comparative example, the pipe with the corrosion-resistant alloy layer coated on the pipe end has a diameter of 60 mm, a wall thickness of (5+2) mm, a groove angle of 52°, and a pair gap of 4 mm.
[0152] The difference from Example 3 is that the filling layer feeding pattern is changed from zigzag to crescent. The welding process and parameters are shown in Table 3. The macroscopic morphology of the cross section of the welded joint is as follows: Fig.26 As shown; the base material and the filling layer form a martensitic structure ( Fig. 27 ); tensile fracture at the interface ( Fig.28 ). According to the NB / T47014-2011 standard bending test, the front bend is intact, but the back bend has cracks ( Fig.29 ).
[0153] Table 3 Welding process and parameters
[0154]
[0155] Comparative Example 4:
[0156] This comparative example provides a pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. In this comparative example, the pipe with the corrosion-resistant alloy layer coated on the pipe end has a diameter of 60 mm, a wall thickness of (5+2) mm, a groove angle of 52°, and a pair gap of 4 mm.
[0157] The difference from Example 3 is that no magnetic hot metal gathering device is installed. The macroscopic morphology of the cross section of the welded joint is as follows: Fig.30 As shown in the figure, the interface between the base material and the filling layer, the filling layer and the cover layer all form a martensitic structure ( Fig.31 and Fig.32 ); tensile fracture at the center of the weld ( Fig.33 ). According to the NB / T47014-2011 standard bending test, cracks appeared in both the front and back bends ( Fig.34 ).
[0158] Embodiment 4:
[0159] This embodiment provides a pipe-to-pipe butt welding process based on Embodiment 2 in which the pipe end is coated with a corrosion-resistant alloy layer. In this embodiment, the pipe end coated with a corrosion-resistant alloy layer has a diameter of 114 mm, a wall thickness of (6+2) mm, a groove angle of 55°, and a pair gap of 4.5 mm.
[0160] Before welding, a magnetic hot metal device was installed. The welding process and parameters are shown in Table 4. The macroscopic morphology of the cross section of the joint after welding is as follows: Fig.35 As shown; no martensite formation was observed at the interface between the parent material and the filling layer, as well as in the filling layer ( Fig.36 After welding with this process and parameters, tensile and bending tests were carried out according to NB / T47014-2011 standard. The tensile fracture was located at the parent material ( Fig.37), bending intact ( Fig.38 The intergranular corrosion of the welded joint was carried out according to GBT 4334-2020 standard. No corrosion pits were found on the weld surface after intergranular corrosion, and the corrosion specimen was intact ( Fig.39 ).
[0161] Table 4 Welding process
[0162]
[0163] Comparative Example 5:
[0164] This comparative example provides a pipe butt welding process with a corrosion-resistant alloy layer coated on the pipe end. In this comparative example, the pipe with the corrosion-resistant alloy layer coated on the pipe end has a diameter of 114 mm, a wall thickness of (5+2) mm, a groove angle of 55°, and a pair gap of 4.5 mm.
[0165] Unlike Example 4, the magnetic hot metal device was not installed, which resulted in the formation of a martensitic structure at the fusion line and filling layer. Fig.40 After welding with this process and parameters, tensile and bending tests were carried out according to NB / T47014-2011 standard. The tensile fracture was located at the fusion line ( Fig.41 ), bending also cracks at the fusion line ( Fig.42 The intergranular corrosion of the welded joint was carried out according to GBT 4334-2020 standard. The intergranular corrosion specimen was bent and cracked ( Fig.43 ).
Claims
1. A pipe-to-pipe butt welding process with a corrosion-resistant alloy layer on the inner end of the pipe. It is characterized in that The process includes the following steps: Step 1: Clean the pipe end: Step 2: Weld joint assembly and spot fixing: Step 3: arranging magnetic molten iron devices at both ends of the pipes: After the weld joint is paired and spot-fixed in step 2, magnetic iron gathering devices are installed at both ends of the groove. The distance between the magnetic iron gathering devices and the groove of the pipe end is 15 to 20 mm. A pair of magnetic iron gathering devices are symmetrically arranged at the pipe ends on both sides, and the side close to the groove is the S pole; Step 4: Base layer welding: The base layer is welded in two half-circles, the base layer is welded by argon arc welding, and the welding wire of argon arc welding is stainless steel argon-free self-shielded welding wire with the same chemical composition as the corrosion-resistant alloy coating. After the base layer is welded, the thickness of the welding layer is 1.4mm~2mm; Step 5: Filling layer welding: The filling layer is welded by arc welding with a welding current of 65 to 80A; After the filling layer is welded, the weld surface should be slightly lower than the upper edge of the groove by 0.5 to 1 mm, keeping the upper edge of the groove in its original state; After the filling layer is welded, the microhardness of the filling layer in the weld cross section should be less than 350Hv; Step 6: Cover layer welding: The cover layer is welded by arc welding with a welding current of 70 to 85A.
2. The pipe-to-pipe butt welding process with the pipe end internally coated with a corrosion-resistant alloy layer as claimed in claim 1, It is characterized in that In step three, the magnetic molten iron gathering device comprises a magnet attractor (1), the magnet attractor comprises an austenitic stainless steel shell (2), a bar magnet seat mounting hole (3) is provided on the austenitic stainless steel shell (2) along the longitudinal direction; chromium-zirconium-copper magnetic isolation blocks (4) are respectively provided on the austenitic stainless steel shell (2) on both sides of the bar magnet seat mounting hole (3) along the longitudinal direction, a bar magnet seat (5) is installed in the bar magnet seat mounting hole (3), a bar magnet (8) and a knob switch (12) are provided on the bar magnet seat (5), the knob switch (12) drives the bar magnet (8) on the bar magnet seat (5) to rotate together in the bar magnet seat mounting hole (3), when the end of the bar magnet (8) is flush with the chromium-zirconium-copper magnetic isolation block (4), the chromium-zirconium-copper magnetic isolation block (4) can isolate the bar magnet (8); A suction opening (6) is arranged longitudinally on the lateral inner side of the austenitic stainless steel shell (2), the opening of the suction opening (6) is laterally away from the bar magnet seat mounting hole (3), the bottom of the suction opening (6) is laterally close to the bar magnet seat mounting hole (3), and a second V-shaped groove (7) arranged longitudinally is opened at the bottom of the suction opening (6), and two groove surfaces of the second V-shaped groove (7) are arranged tangentially to the suction opening (6); A permanent magnet (9) is arranged on one side of the austenitic stainless steel shell (2) near the groove, the permanent magnet (9) is a semicircular ring structure, and the inner diameter of the permanent magnet (9), the inner diameter of the suction opening (6) and the radius of the pipe (14) to be butt-welded are the same; A first magnetic isolation sheet (10) made of austenitic stainless steel is provided between the permanent magnet (9) and the magnetic attractor (1); The vertical upper and lower parts of the semicircular openings of the magnetic attractor (1) and the permanent magnet (9) are respectively provided with austenitic stainless steel second magnetic isolation plates (11).
3. The pipe-to-pipe butt welding process with the pipe end coated with a corrosion-resistant alloy layer as claimed in claim 1, It is characterized in that The pipe fitting (14) to be butt-welded has a pipe diameter of 60 to 114 mm, a pipe wall thickness of 5 to 6 mm, and a corrosion-resistant alloy layer thickness of 1.5 to 2 mm.
4. The pipe-to-pipe butt welding process with a pipe end coated with a corrosion-resistant alloy layer as claimed in claim 1, It is characterized in that The specific process of step one is: use a straight-shank angle grinder equipped with a handle flap wheel cylindrical grinding head to grind the outer wall of the pipe end with a groove within 20 to 30 mm to expose the metallic luster, and then use a straight-shank angle grinder equipped with a handle brown corundum conical grinding wheel grinding head to clean the inner wall of the pipe end within 15 to 20 mm.
5. The pipe-to-pipe butt welding process with the pipe end internally coated with a corrosion-resistant alloy layer as claimed in claim 1, It is characterized in that The specific process of step 2 is: placing the two tube ends covered with the corrosion-resistant alloy layer in the first V-shaped groove (13) prepared in advance for pairing, with a pairing gap of 3.0-4.5 mm; after the pairing is completed, the two tube ends are spot-fixed by argon arc welding in a free state, with a spot-fixing length of 8-10 mm.
6. The pipe-to-pipe butt welding process with the pipe end internally coated with a corrosion-resistant alloy layer as claimed in claim 5, It is characterized in that In step 2, the first V-shaped groove (13) is a pairing device formed by welding two identical pipes together at the outer wall generatrix, and the length is 500 to 600 mm. The diameter of a single pipe of the first V-shaped groove (13) is 1.5 to 2 times the diameter of the pipe (14) to be butt-welded.
7. The pipe-to-pipe butt welding process with the pipe end internally coated with a corrosion-resistant alloy layer as claimed in claim 5, It is characterized in that In step 2, the argon arc welding machine is a plug-in and rechargeable dual-purpose welding machine that integrates electrode arc welding and argon arc welding.
8. The pipe-to-pipe butt welding process with the pipe end internally coated with a corrosion-resistant alloy layer as claimed in claim 1, It is characterized in that The method further includes: Step 7, post-weld treatment: Step 8: Appearance inspection: Step 9, Rework: The welding process from step 1 to step 7 is used to perform repair welding of the pipe fitting.
9. A magnetic molten iron device, It is characterized in that The invention comprises a magnet attractor (1), wherein the magnet attractor comprises an austenitic stainless steel shell (2), a strip magnet seat mounting hole (3) is provided on the austenitic stainless steel shell (2) along the longitudinal direction; chromium-zirconium-copper magnetic isolation blocks (4) are respectively provided on the austenitic stainless steel shell (2) on both sides of the strip magnet seat mounting hole (3) along the longitudinal direction; a strip magnet seat (5) is installed in the strip magnet seat mounting hole (3); a strip magnet (8) and a knob switch (12) are provided on the strip magnet seat (5); the knob switch (12) drives the strip magnet (8) on the strip magnet seat (5) to rotate together in the strip magnet seat mounting hole (3); when the end of the strip magnet (8) is flush with the chromium-zirconium-copper magnetic isolation block (4), the chromium-zirconium-copper magnetic isolation block (4) can isolate the strip magnet (8); A suction opening (6) is arranged longitudinally on the lateral inner side of the austenitic stainless steel shell (2), the opening of the suction opening (6) is laterally away from the bar magnet seat mounting hole (3), the bottom of the suction opening (6) is laterally close to the bar magnet seat mounting hole (3), and a second V-shaped groove (7) arranged longitudinally is opened at the bottom of the suction opening (6), and two groove surfaces of the second V-shaped groove (7) are arranged tangentially to the suction opening (6); A permanent magnet (9) is arranged on one side of the austenitic stainless steel shell (2) near the groove, the permanent magnet (9) is a semicircular ring structure, and the inner diameter of the permanent magnet (9), the inner diameter of the suction opening (6) and the radius of the pipe (14) to be butt-welded are the same; A first magnetic isolation sheet (10) made of austenitic stainless steel is provided between the permanent magnet (9) and the magnetic attractor (1); The vertical upper and lower parts of the semicircular openings of the magnetic attractor (1) and the permanent magnet (9) are respectively provided with austenitic stainless steel second magnetic isolation plates (11).