Method for preventing bamboo tableware from cracking
By using a combination of adipic acid and citric acid as a crosslinking agent, the fiber bonding strength of bamboo tableware is enhanced through esterification, solving the problem of cracking in bamboo tableware and significantly improving its durability.
Patent Information
- Application Number
- CN202411051923.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-08
AI Technical Summary
Bamboo tableware is prone to cracking after a period of use. Existing technology has failed to effectively enhance the bonding strength of bamboo fibers, resulting in insufficient durability.
A combination of dicarboxylic acids, such as adipic acid and citric acid, is used as a crosslinking agent. Through soaking, heat preservation baking and natural cooling, the carboxylic acid molecules undergo an esterification reaction with bamboo cellulose and lignin macromolecules, thereby enhancing the fiber bonding strength.
It significantly improves the durability of bamboo tableware, reduces cracking, and enhances the horizontal bonding strength of bamboo fibers.
Smart Images

Figure BDA0004975164330000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bamboo product processing, and in particular relates to a method for preventing bamboo tableware from cracking. Background Art
[0002] Bamboo is a natural material with low production cost and abundant resources. Bamboo products made of bamboo are harder than wood, have a longer expected service life than wood, and have a natural smell, exuding a fresh and fragrant smell, which is beneficial to physical and mental health. However, daily bamboo products, such as bamboo tableware, are prone to dehydration and cracking after being used for a period of time. Therefore, in addition to improving the manufacturing process of bamboo products, it is also important to adopt certain methods to enhance the connection strength of bamboo fibers. The present invention provides a method for preventing bamboo tableware from cracking and describes its specific steps.
[0003] Dibasic or polybasic acids are important raw materials for a variety of chemicals and are widely used in chemical industry. Among them, adipic acid and citric acid are almost non-toxic and are common food additives. Adipic acid and citric acid molecules contain two or more carboxyl groups and have good esterification reaction activity. At a certain temperature, the carboxyl groups in the carboxylic acid molecules are easy to react with the hydroxyl groups of macromolecular compounds such as cellulose and lignin in bamboo fiber to undergo a series of complex esterification cross-linking reactions. After the reaction is carried out for a long enough time, most of the carboxylic acid molecules can be connected to the surrounding macromolecules such as cellulose through the ester group.
[0004] Bamboo contains a large amount of high-polysaccharides such as cellulose, and most of its molecules run along the natural growth direction of bamboo, that is, the vertical direction, which can be reflected in the form of strips of bamboo fibers on a macro scale. When dibasic or polybasic carboxylic acid molecules are roughly connected to two macromolecules such as cellulose in the horizontal direction, the connection strength of bamboo fibers is enhanced, and cracks in the vertical direction are less likely to occur than in normal cases. Summary of the invention
[0005] The problem to be solved by the present invention is to overcome the shortcoming that bamboo tableware is easy to crack, provide a method to prevent the bamboo tableware from cracking, effectively enhance the connection strength between bamboo fibers of the bamboo tableware, and improve the durability of the bamboo tableware.
[0006] In order to solve the above problem, the technical solution provided by the present invention is: a method for preventing bamboo tableware from cracking, the method comprising the following steps:
[0007] (1) Soak the bamboo tableware in a certain volume of crosslinking agent aqueous solution for 12 to 48 hours;
[0008] (2) Drain the soaked bamboo tableware and bake it for 0.5 to 5 hours;
[0009] (3) After baking, place the bamboo tableware at room temperature to cool naturally;
[0010] (4) After cooling, wash the bamboo tableware in clean water and then place it in a cool place to dry naturally.
[0011] The bamboo tableware in step (1) is taken from one of moso bamboo, nan bamboo, purple bamboo, square bamboo, cotton bamboo, hemp bamboo, ci bamboo, indigo bamboo, fragrant bamboo, green bamboo and green bamboo.
[0012] The insulation temperature in step (1) is 50°C to 100°C.
[0013] The crosslinking agent in step (1) is a composition of dibasic or polybasic carboxylic acids.
[0014] Furthermore, the cross-linking agent in step (1) is a combination of adipic acid and citric acid.
[0015] Furthermore, the mass ratio of adipic acid solution to citric acid in the cross-linking agent in step (1) is 1:15 to 15:1.
[0016] Furthermore, the mass concentration of the cross-linking agent aqueous solution in step (1) is 5% to 50%.
[0017] Furthermore, the crosslinking agent aqueous solution in step (1) is 2 to 20 times the weight of the bamboo tableware.
[0018] Furthermore, the insulation temperature in step (2) ranges from 90°C to 175°C.
[0019] The present invention has the following advantages: the raw materials adipic acid or citric acid involved in the method shown in the present invention are relatively cheap and almost non-toxic to human body and environment, and can be promoted on a large scale.
[0020] The beneficial effects of the present invention are:
[0021] The method described in the present invention uses dibasic or polybasic carboxylic acid molecules and macromolecules containing a large number of hydroxyl groups such as cellulose and lignin in bamboo to fully undergo a series of reactions such as esterification at a certain temperature. With dibasic or polybasic carboxylic acids as the medium, the connection between macromolecules such as cellulose and lignin is strengthened at the molecular level, and the connection strength between cell walls inside bamboo is strengthened, thereby strengthening the connection strength of bamboo fibers in the horizontal direction at the macro level, and significantly improving the durability of bamboo tableware. Specific implementation methods
[0023] Example 1
[0024] (1) 10 identical bamboo cups (10 cm in height, 6 cm in inner diameter, 0.5 cm in wall thickness) made of moso bamboo were selected and immersed in a 10-liter crosslinking agent aqueous solution composed of adipic acid and citric acid, wherein the total mass concentration of the crosslinking agent was 20%, wherein the mass concentrations of adipic acid and citric acid were 2% and 18%, respectively; and the mixture was immersed at 80°C for 24 h;
[0025] (2) Drain the soaked bamboo cups and bake them at 160°C for 2 hours;
[0026] (3) After baking, place the bamboo cup at room temperature to cool naturally;
[0027] (4) After cooling, wash the bamboo cup in clean water and then place it in a cool place to dry naturally.
[0028] Embodiments 2 to 9
[0029] The total mass concentration of adipic acid and citric acid is controlled to be 20% of the solution, and the mass concentrations of adipic acid and citric acid in the crosslinking agent aqueous solution of step (1) of Example 1 are adjusted. The remaining implementation steps are in accordance with Example 1. The bamboo age and the size of the bamboo cup are the same as those in Example 1.
[0030] Embodiments 10 to 12
[0031] The total mass concentration of the crosslinking agent aqueous solution in step (1) of Example 1 was adjusted to 10%, 30%, and 40%, respectively, and the corresponding mass concentration ratios of adipic acid and citric acid were adjusted to 5%:5%, 15%:15%, and 20%:20%, respectively. The remaining implementation steps were the same as in Example 1, and the bamboo age and the size of the bamboo cup were the same as in Example 1.
[0032] Embodiments 13-14
[0033] The baking temperatures in step (2) of Example 1 were adjusted to 100° C. and 130° C. respectively. The remaining implementation steps were the same as those of Example 1, and the age of the bamboo and the size of the bamboo cup were the same as those of Example 1.
[0034] Comparative Example 1
[0035] (1) 10 bamboo cups made of moso bamboo were selected. The bamboo age and the size of the bamboo cups were the same as those in Example 1. The cups were immersed in 10 liters of 20% citric acid aqueous solution at 80° C. for 24 hours.
[0036] (2) Drain the soaked bamboo cups and bake them at 160°C for 2 hours;
[0037] (3) After baking, place the bamboo cup at room temperature to cool naturally;
[0038] (4) After cooling, wash the bamboo cup in clean water and then place it in a cool place to dry naturally.
[0039] Comparative Example 2
[0040] (1) 10 bamboo cups made of moso bamboo were selected. The bamboo age and the size of the bamboo cups were the same as those in Example 1. The cups were immersed in 10 liters of a 20% adipic acid aqueous solution at 80° C. for 24 hours.
[0041] (2) Drain the soaked bamboo cups and bake them at 160°C for 2 hours;
[0042] (3) After baking, place the bamboo cup at room temperature to cool naturally;
[0043] (4) After cooling, wash the bamboo cup in clean water and then place it in a cool place to dry naturally.
[0044] Blank control group
[0045] (1) 10 bamboo cups made of moso bamboo were selected. The bamboo age and the size of the bamboo cups were the same as those in Example 1. The cups were soaked in 10 liters of water at 80° C. for 24 hours.
[0046] (2) Drain the soaked bamboo cups and bake them at 160°C for 2 hours;
[0047] (3) After baking, place the bamboo cup at room temperature to cool naturally;
[0048] (4) After cooling, wash the bamboo cup in clean water and then place it in a cool place to dry naturally.
[0049] Bamboo cup durability test
[0050] The following experiments further illustrate that the method demonstrated by the present invention has the effect of preventing the bamboo cup from cracking, and compared with the cross-linking agent aqueous solution prepared by using adipic acid or citric acid alone, the cross-linking agent aqueous solution prepared by adipic acid and citric acid has a better effect, and the optimal ratio of the mass fractions of adipic acid and citric acid is further screened.
[0051] Take 170 bamboo cups made of bamboo (10 cm high, 6 cm inner diameter, 0.5 cm wall thickness), and randomly and evenly divide them into 17 identical groups. They are Comparative Example 1, Comparative Example 2, Examples 1 to 14, and a blank control group. Treat each group of bamboo cups according to each comparative example and example. Place the treated bamboo cups in an oven at 200°C and bake, and adjust the oven temperature to slowly rise from room temperature to the set temperature. Record the baking time when obvious cracks appear on each bamboo cup in each group. Obtain the median time when cracks appear on the bamboo cups in each group and record them. The experimental results are shown in Table 1 below:
[0052] Table 1. Baking time of bamboo cups until cracking in examples and comparative examples
[0053]
[0054] From the above test results, it can be seen that compared with the blank control group, the durability of the bamboo cups in each group of embodiments has increased significantly, and the cracking time of the bamboo cups can reach up to 18.1h. By comparing the experimental results of Example 5 with those of Examples 13-14, it can be seen that increasing the baking temperature can increase the time for cracks to appear in the bamboo cups, and the durability of the bamboo cups is enhanced. By comparing Example 5 with Examples 10-12, it can be seen that increasing the concentration of the crosslinking agent aqueous solution in which the bamboo cups are soaked can significantly improve the durability of the bamboo cups, making the bamboo cups less likely to crack. By comparing Examples 1-9 with Comparative Examples 1-2, it can be seen that when the mass concentration ratio of adipic acid and citric acid is 10.0%:10.0%, the bamboo cups are least likely to crack. Compared with the use of adipic acid or citric acid aqueous solution alone, the crosslinking agent aqueous solution prepared by adipic acid and citric acid has a better effect. After being soaked and heat-insulated and baked in adipic acid or citric acid solution or a solution prepared by the two, the bamboo cups are less likely to crack. Therefore, this treatment method can effectively prevent the cracking of bamboo cups.
Claims
1. A method to prevent bamboo tableware from cracking. It is characterized in that The method comprises the following steps: (1) Soaking bamboo tableware in a crosslinking agent aqueous solution, wherein the crosslinking agent is a composition of a dibasic or polybasic carboxylic acid, and the crosslinking agent aqueous solution is 2 to 20 times the weight of the bamboo tableware, and the soaking time is 12 to 48 hours; (2) Drain the soaked bamboo tableware and bake it for 0.5 to 5 hours; (3) After baking, place the bamboo tableware at room temperature to cool naturally; (4) After cooling, wash the bamboo tableware in clean water and then place it in a cool place to dry naturally.
2. The method according to claim 1, Features: The bamboo tableware in step (1) is made of one of moso bamboo, nan bamboo, purple bamboo, square bamboo, cotton bamboo, hemp bamboo, ci bamboo, indigo bamboo, fragrant bamboo, green bamboo and green bamboo.
3. The method according to claim 1, Features: The insulation temperature in step (1) is 50°C to 100°C.
4. The method according to claim 1, Features: The mass ratio of the adipic acid solution to the citric acid is 1:15 to 15:
1.
5. The method according to claim 1, Features: The mass concentration of the crosslinking agent aqueous solution in step (1) is 5% to 50%.
6. The method according to claim 1, Features: The crosslinking agent aqueous solution in step (1) is 2 to 20 times the weight of the bamboo tableware.
7. The method according to claim 1, Features: The insulation temperature in step (2) ranges from 90°C to 175°C.