Rubber composite material bonding interface integration method
Through the rubber composite material combined with interface integration method, the adhesive process of plasma surface treatment reinforcement layer and wear-resistant layer is used, combined with the combination of high-modulus glass fiber, carbon fiber and aramid fiber, the high energy consumption of existing metal scrapers is solved. and unsustainability issues, efficient and low-cost scraper design has been achieved, meeting the rigidity, wear resistance and lightweight requirements of scraper in the coal mining industry.
Patent Information
- Application Number
- CN202410974457.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Existing metal scraper components have high energy consumption, high cost and unsustainability problems in the coal mining industry. The non-metallic scraper design has not yet met market demand, and there is a lack of alternative solutions to meet the rigidity and wear resistance requirements.
Using the rubber composite material combined with interface integration method, the adhesive process between the plasma surface treatment reinforcement layer and the wear-resistant layer is formed, and the structure of foam layer, continuous fiber reinforcement composite reinforcement layer and wear-resistant layer is used to utilize high-modulus glass The combination of fiber, carbon fiber and aramid fiber combines aramid pulp rubber elastomer wear-resistant layer to improve bonding strength and material properties.
It significantly improves the overall stiffness and impact resistance of the scraper, reduces the number of fiber layers, realizes rapid molding of complex shapes and the integration of fiber-reinforced foam sandwich structure, significantly improves the bonding strength and cost-effectiveness, and meets the mineral use Requirements for strength, stiffness and wear resistance of non-metallic scrapers.
Smart Images

Figure CN118906488A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of machinery, in particular to a method for integrating a rubber composite material bonding interface. Background Art
[0002] As the main transportation device and transportation track for mining coal resources, the design and reliability of the scraper conveyor directly affect the comprehensive collection efficiency of the coal mine system. At present, the research on scraper conveyors mainly focuses on their power, life, safety and applicability under various working conditions, among which the structural design optimization and upgrading of the scraper conveyor itself have received great attention. As an important component, the lightweight and high-strength scraper components will reduce the production cost of coal mine operations, reduce system transportation power consumption and sprocket wear; the efficient scraper component design can reduce scraper damage and the reserve of replacement parts, thereby reducing the company's production management costs and increasing the service life of the scraper conveyor.
[0003] At present, scraper components made of alloy structural steel have been widely used, but due to the high energy consumption, high cost and unsustainability of metal scraper components, the coal mining industry has been exploring alternatives to metal scrapers. Existing research mainly focuses on the design ideas of non-metallic scraper blades, but there is still no non-metallic material on the market that can meet market demand. The composite scraper of the present invention adopts the design concept of regional division, refines the performance requirements of each part of the scraper component, and meets the stiffness and wear resistance requirements of the composite scraper through structural and material matching. The present invention provides a rubber composite material combined interface integration method to provide new design ideas for expanding the collection of composite materials. Summary of the invention
[0004] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a method for integrating the bonding interface of a rubber composite material. By using a plasma surface treatment bonding process between the reinforcing layer and the wear-resistant layer, the surface roughness can be significantly increased and active groups can be retained. These active groups can chemically bond with the adhesive during bonding and significantly improve the bonding strength.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for integrating a rubber composite material bonding interface. The rubber composite material comprises, from the inside to the outside: a foam layer, a continuous fiber reinforced composite material reinforcement layer wrapped outside the foam layer, and a wear-resistant layer wrapped outside the continuous fiber reinforced composite material reinforcement layer; the continuous fiber reinforced composite material reinforcement layer consists of an inner layer, a center layer, and an outer layer; the inner layer is high modulus glass fiber, the center layer is carbon fiber, and the outer layer is aramid fiber; the wear-resistant layer is an aramid pulp rubber elastomer wear-resistant layer; a plasma method is used to perform plasma surface treatment on the surface of the wear-resistant layer, and then the wear-resistant layer is connected to the continuous fiber reinforced composite material reinforcement layer.
[0007] The aforementioned method for integrating the rubber composite material with the interface comprises the following steps:
[0008] Step 1: embed the metal embedded parts that match the beam bolts into the foam to form a foam layer;
[0009] Step 2, integrating the foam layer with the high modulus glass fiber, the carbon fiber and the aramid fiber by molding;
[0010] Step 3, injecting resin into the structure of step 2 and curing it to form a continuous fiber reinforced composite material reinforcement layer to form an integrated material as a whole;
[0011] Step 4: using plasma surface treatment to treat the contact surface between the reinforcement layer and the wear-resistant layer of the continuous fiber reinforced composite material;
[0012] Step 5: Use installation glue to glue the two sides of the structure of the integrated material in blocks;
[0013] Step 6: Press and assemble the split wear-resistant layer and the integrated material, then perform high-temperature isostatic treatment to eliminate residual stress, and finally let it stand and wait for natural failure to obtain a rubber composite material.
[0014] In the aforementioned rubber composite material bonding interface integration method, the injection pressure range of the resin in step three is: 50-300 bar, preferably: 100 bar.
[0015] In the aforementioned rubber composite material combined with the interface integration method, the resin injection mold in step three adopts an upper and lower mold design, and is locked and opened by a press. The injection gun head is directly embedded in the mold, and the injection gun head adopts a self-cleaning design.
[0016] In the aforementioned rubber composite material bonding interface integration method, the curing time of the resin in step three is 10-15 minutes.
[0017] The aforementioned method for integrating the interface of a rubber composite material, step four: installing the integrated material on a fixed stand, and using a six-axis robot arm equipped with a plasma surface treatment contact to perform fully automatic surface treatment to activate the contact surface between the wear-resistant layer and the continuous fiber reinforced composite material.
[0018] The aforementioned method for integrating the interface of a rubber composite material, step five: using a six-axis robot arm with a glue contact head installed, the contact surface of the integrated material is subjected to a fully automatic glue assembly process, and both sides of the structure are glued in blocks.
[0019] The present invention is beneficial in that:
[0020] The thick non-metal scraper structure adopts the foam sandwich composite material design, which effectively improves the overall stiffness and impact resistance while reducing the fiber layer and ensuring the assembly of peripheral parts; through the rapid molding process, the rapid prototyping of complex composite materials and the integrated preparation of fiber-reinforced foam sandwich structures are realized;
[0021] The present invention surprisingly found that plasma treatment improves rubber viscosity, and the plasma surface treatment bonding process between the reinforcement layer and the wear-resistant layer can significantly increase the surface roughness and leave active groups, which can chemically bond with the adhesive during bonding and significantly improve the bonding strength. This discharge equipment is reasonably priced, and the dielectric barrier discharge can stably generate a continuous plasma source at normal temperature and pressure, ensuring the bonding continuity and cost advantage of this integrated technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a structural schematic diagram of an embodiment of the present invention;
[0023] Figure 2 is the AFM spectrum of the CFRP surface before and after the plasma treatment of the present invention;
[0024] Figure 3 Schematic diagram of contact angle of the present invention;
[0025] Figure 4 Graphs showing the test results of improving rubber viscosity by plasma treatment of the present invention ((a) polytetrafluoroethylene / polydimethylsiloxane / Cu, (b) polytetrafluoroethylene / polydimethylsiloxane / SUS430, (c) polytetrafluoroethylene / polydimethylsiloxane / glass);
[0026] 1 non-metal scraper, 101 foam layer, 102 metal embedded parts, 103 continuous fiber reinforced composite material reinforcement layer, 104 wear-resistant layer. DETAILED DESCRIPTION
[0027] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] The non-metal scraper 1 for mining includes: a foam layer 101, a metal embedded part 102 embedded in the foam layer 101, a continuous fiber reinforced composite material reinforcement layer 103 integrally formed with the foam layer 101 and wrapped outside the foam layer 101, and a wear-resistant layer 104 wrapped outside the continuous fiber reinforced composite material reinforcement layer 103. The foam layer 101 includes: a PVC foam layer 101, a PET foam layer 101, an MPPE foam layer 101, a PMI foam layer 101 or a PU foam layer 101. The foam layer 101 is designed as an inner liner to achieve the effect of compatibility between lightweight and high rigidity.
[0029] The continuous fiber reinforced composite reinforcement layer 103 is composed of an integrated material structure of fiber plies and resin injection and curing. The fiber plies are: the inner layer is a woven cloth or plain cloth of high modulus glass fiber, the center layer is a woven cloth or plain cloth of carbon fiber, and the outer layer is a woven cloth or plain cloth of aramid fiber. The weight ratio of the woven cloth or plain cloth of high modulus glass fiber is 40%, the weight ratio of the woven cloth or plain cloth of carbon fiber is 40%, and the weight ratio of the woven cloth or plain cloth of highly wear-resistant aramid fiber is 20%. The fibers of the fiber-reinforced composite material are initially selected from high modulus glass fiber and carbon fiber, and the density of carbon fiber is generally 1.7-1.8g / cm 3 , tensile strength is 3000-5000MPa, elastic modulus is 200-400Gpa; density of glass fiber is generally 2.5-3.0g / cm 3 , tensile strength is 1000~3000MPa, elastic modulus is close to 100Gpa. Therefore, in order to ensure sufficient rigidity of the scraper components and achieve lightweight and low cost of the scraper, the fiber selection needs to adopt a mixed layering method of glass fiber and carbon fiber.
[0030] The wear-resistant layer 104 includes: a zirconia ceramic layer, an alumina-zirconia composite ceramic layer, a carbon / carbon composite material layer, a carbon fiber reinforced carbon-based composite material layer, a steel material layer, a 40Mn2 steel layer, an aramid fiber reinforced mixed rubber polymer composite material layer, an aramid canvas rubber skeleton layer or an aramid pulp rubber elastomer layer; as a preferred embodiment, it is an aramid pulp rubber elastomer layer. Aramid pulp rubber elastomer has the characteristics of excellent dispersibility and good compatibility with rubber matrix materials. Aramid pulp can be added to natural rubber, hydrogenated nitrile rubber, chloroprene rubber, fluororubber, silicone rubber, styrene-butadiene rubber, isoprene rubber, and chloroprene rubber, which can achieve the following effects: a) increase the tear resistance and friction resistance of the matrix material; b) increase the shear resistance of the matrix c) greatly improve the modulus under low strain; d) increase the hardness.
[0031] 1. A method for integrating a rubber composite material with an interface, comprising the following steps:
[0032] Step 1: embed the metal embedded parts that match the beam bolts into the foam to form a foam layer;
[0033] Step 2, integrating the foam layer with the high modulus glass fiber, the carbon fiber and the aramid fiber by molding;
[0034] Step 3, injecting resin into the structure of step 2 and curing it to form a continuous fiber reinforced composite material reinforcement layer to form an integrated material as a whole;
[0035] The molding of thick foam sandwich composite materials is initially planned to be a liquid resin molding curing process or a prepreg cladding autoclave molding process. In order to improve the molding process efficiency and quality of variable cross-section and thick frame side beams, the proposed methods include the following:
[0036] a) Reduce the resin infiltration time
[0037] The process of resin impregnation of fiber preform can be approximately regarded as the permeation behavior of fluid in porous media, which follows Darcy's law:
[0038]
[0039] Where V is the speed of resin infiltration, Q is the total resin injection volume, A flow It is the cross-sectional area of resin flow. K is the permeability of the preform, dp / dx is the pressure in the mold, and η is the viscosity of the resin. Within the research scope of this project, K is regarded as a fixed constant under the premise that the preform is fixed. Therefore, the factors affecting the die time are resin viscosity and pressure difference. The viscosity of epoxy resin generally decreases to a certain extent with increasing temperature, but considering other comprehensive factors, the choice of resin is limited. Therefore, the injection pressure is mainly increased to increase the infiltration speed and reduce the infiltration time. As a preferred embodiment, the injection pressure range of the resin is: 50-300bar, and further preferred: 100bar.
[0040] b) Reduce mold assembly time. Currently, low-pressure molds are split mold designs, and mold assembly is cumbersome. They also require connection joints, vacuum pipes, and other work, which takes a long time. The new solution proposes to adopt an upper and lower mold design, with a press for mold locking and mold opening, to simplify the mold assembly process. The injection gun head is directly embedded in the mold, and the injection gun head adopts a self-cleaning design. After the injection is completed, there is no need to clean the gun head, realizing continuous production.
[0041] c) Reduce the curing time;
[0042] There are two main aspects to consider in reducing the curing time: reducing the curing time of the resin; reducing the time for heating and cooling the mold; the curing time of the resin is mainly determined by the resin selection. According to the curing principle of epoxy resin, in general, the curing time is inversely proportional to the process opening time, and the shorter the process opening time requirement, the faster the curing time, and vice versa. Therefore, the premise of shortening the curing time is to reduce the process opening time, that is, to increase the resin injection speed. Therefore, after reducing the injection time by the method described above, a relatively fast curing resin can be selected. The curing time of the resin is 10-15 minutes.
[0043] For the traditional RTM process, the mold is generally heated by an oven, which has low heating efficiency, long heating time and high energy consumption. This solution proposes to use an oil temperature machine for heating, and the mold is equipped with a heating oil circuit. The heating efficiency is high and the energy consumption is low. At the same time, the high-temperature injection method is used, and the mold does not need to be repeatedly heated and cooled, which reduces the cycle time.
[0044] d) Reduce demoulding and mold cleaning time
[0045] The traditional low-pressure RTM process uses a two-component resin system and uses an external release agent for demoulding. The external release agent has a good demoulding effect, but it needs to be sprayed frequently, which will cause the external release agent to remain, resulting in the need for frequent mold cleaning.
[0046] The resin adopts toughened epoxy resin of Huibo resin.
[0047] e) Use equipment with a high degree of automation to ensure process stability and consistency of product quality.
[0048] The high-pressure injection process and the press pressing process are mostly automated, which reduces the instability caused by human factors in the process and ensures the stability of part quality.
[0049] Step 4: Install the integrated material on a fixed stand and use a six-axis robot equipped with a plasma surface treatment contact to perform fully automatic surface treatment to activate the contact surface between the wear-resistant layer and the continuous fiber reinforced composite material.
[0050] Step 5: Use a six-axis robot arm with a glue contact head to perform a fully automatic glue assembly process on the contact surface of the integrated material, and glue the two sides of the structure in blocks.
[0051] Step 6: Press and assemble the split wear-resistant layer and the integrated material, then perform high-temperature isostatic treatment to eliminate residual stress, and finally let it stand and wait for natural failure to obtain a rubber composite material.
[0052] The resin injection mold adopts an upper and lower mold design, and is equipped with a press to lock and open the mold. The injection gun head is directly embedded in the mold, and the injection gun head adopts a self-cleaning design.
[0053] 2. Verification experiment: Analysis of the impact of plasma surface treatment on product quality:
[0054] The surface is treated by plasma using a plasma method.
[0055] The CFRP bonding surface was pretreated by air plasma at room temperature and pressure. After treatment, the contact angle between CFRP and water was reduced and the surface energy of CFRP was 32.49mJ / m 2 After plasma treatment, its surface energy increased to 54.39mJ / m 2, and the polar surface energy is significantly increased. At the same time, the epoxy functional groups on the CFRP surface are enhanced, the surface roughness is increased, and a large number of micron-scale grooves are formed on the surface (such as Figure 2 As shown in the figure, the tensile shear strength of epoxy resin adhesive joints is significantly improved, and its failure mode is transformed from interface failure to substrate failure.
[0056] Carbon fiber reinforced epoxy resin composites (CF / EP) were sprayed by low-temperature plasma and their effects on bonding properties were studied. The results show that the treatment effect of low-temperature plasma surface treatment on CF / EP joints is better than that of traditional sandblasting. After low-temperature plasma surface treatment, the tensile shear strength of CF / EP single lap joints increased by 119.59%, and the failure mode of the joint changed from untreated interface failure to mixed failure dominated by cohesive failure.
[0057] The results of previous experiments have shown that atmospheric plasma surface treatment can effectively improve the surface energy of peroxide-cured fluororubber and reduce its surface contact angle (such as Figure 3 As shown in the figure, it effectively improves the direct bonding strength of peroxide-cured fluororubber, and the tensile strength is increased from 7.3MPa to 12.9MPa.
[0058] The plasma treatment method not only makes vulcanized rubber and polytetrafluoroethylene (PTFE) adhere to each other, but also makes them adhere to other materials. Silicone rubber mainly refers to polydimethylsiloxane (PDMS). The surface is bombarded with a plasma jet to break the silicon-carbon bonds on the surface of the material and convert them into silanols. The newly generated silanols have stronger surface activity. Under high pressure conditions, silanols form hydrogen bonds with oxygen-containing functional groups in the treated PTFE, thereby forming a strong adhesive effect.
[0059] What is more noteworthy is that when the back side of PDMS is also treated with plasma surface, it can also bond with copper and even glass, such as Figure 4 As shown. Compared with the untreated sample, the number of peaks and gullies on the rubber surface increased significantly; the bonding strength of the untreated fluororubber was 561N·m-1. After Ar, air, and O2 plasma treatment, the bonding strength of fluororubber and PTFE increased to 605, 590, and 582N·m-1, respectively. This shows that plasma treatment can greatly improve the bonding performance of rubber.
[0060] In summary: the present invention adopts specific materials with special structures to overcome the defects of single materials, so that the materials and structures form a synergistic effect, meeting the strength, rigidity, wear resistance and lightweight requirements of non-metallic scrapers for mining; the plasma surface treatment bonding process is used between the reinforcing layer and the wear-resistant layer, which can significantly increase the surface roughness and leave active groups. These active groups can chemically bond with the adhesive during bonding and significantly improve the bonding strength. This discharge equipment is reasonably priced, and the dielectric barrier discharge can stably generate a continuous plasma source at normal temperature and pressure, ensuring the bonding continuity and cost advantage of this integrated technology.
[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A method for integrating a rubber composite material with an interface, It is characterized in that The rubber composite material includes, from the inside to the outside: a foam layer, a continuous fiber reinforced composite material reinforcement layer wrapped outside the foam layer, and a wear-resistant layer wrapped outside the continuous fiber reinforced composite material reinforcement layer; the continuous fiber reinforced composite material reinforcement layer consists of an inner layer, a center layer, and an outer layer; the inner layer is high modulus glass fiber, the center layer is carbon fiber, and the outer layer is aramid fiber; the wear-resistant layer is an aramid pulp rubber elastomer wear-resistant layer; the surface of the wear-resistant layer is subjected to plasma surface treatment by a plasma method, and then connected to the continuous fiber reinforced composite material reinforcement layer.
2. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The steps include: Step 1: embed the metal embedded parts that match the beam bolts into the foam to form a foam layer; Step 2, integrating the foam layer with the high modulus glass fiber, the carbon fiber and the aramid fiber by molding; Step 3, injecting resin into the structure of step 2 and curing it to form a continuous fiber reinforced composite material reinforcement layer to form an integrated material as a whole; Step 4: using plasma surface treatment to treat the contact surface between the reinforcement layer and the wear-resistant layer of the continuous fiber reinforced composite material; Step 5: Use installation glue to glue the two sides of the structure of the integrated material in blocks; Step 6: Press and assemble the split wear-resistant layer and the integrated material, then perform high-temperature isostatic treatment to eliminate residual stress, and finally let it stand and wait for natural failure to obtain a rubber composite material.
3. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The injection pressure range of the resin in step 3 is 50-300 bar, preferably 100 bar.
4. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The resin injection mold in the step three adopts an upper and lower mold design, and is equipped with a press to lock and open the mold. The injection gun head is directly embedded in the mold, and the injection gun head adopts a self-cleaning design.
5. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The curing time of the resin in step 3 is 10-15 minutes.
6. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The fourth step is to install the integrated material on a fixed stand and use a six-axis robot equipped with a plasma surface treatment contact to perform fully automatic surface treatment to activate the contact surface between the wear-resistant layer and the continuous fiber reinforced composite material.
7. A rubber composite material bonding interface integration method according to claim 1, It is characterized in that The step five: using a six-axis robot arm with a glue contact head installed to perform a fully automatic glue assembly process on the contact surface of the integrated material, and gluing the two sides of the structure in blocks.