Composite material preparation method, composite material and electronic equipment
The preforming and molding method of profiling tooling is solved, and the problem of glue lack and cracking of fiber materials in complex bending structures is improved, the yield rate and structural integrity of composite materials are improved, and the process flow is simplified.
Patent Information
- Application Number
- CN202411414119.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the preparation of fiber materials, especially in special-shaped parts with complex bending structures, prepregs are prone to deficiencies such as glue deficiency and cracking during the molding process. Especially for special-shaped parts with thinner thicknesses, due to insufficient resin, the resulting The fiber thickness remains unchanged and the resin is pulled laterally in the bent position.
The prepreg is preformed using a profiling tool to form a preform, and then molded in the mold. During preforming, it is heated and softened and solidified to form a set structure to ensure that the resin does not detach from its original position in the bending position and avoids glue deficiency and cracking. Fully heat and vacuum during molding to ensure full bonding of fibers and resin.
By combining preforming and molding, the yield of composite materials is significantly improved, glue deficiency and cracking in the bending position is avoided, and the integrity of complex structures and the correct molding of high-deep and large-curvature structures are ensured. Simple, easy to operate.
Smart Images

Figure CN118906498A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of material preparation, and more specifically, to a composite material preparation method, a composite material and an electronic device. Background Art
[0002] In the related art, fiber material products are usually prepared into prepregs during the preparation process, and then the prepregs are compression molded in a mold. When preparing special-shaped parts with complex bending structures, prepregs are prone to defects during hot pressing. Especially when preparing thin special-shaped parts, during the compression molding process, since there is less resin on the surface of the prepreg, the thickness of the fiber usually does not change when bending, which causes the resin on the outside of the bending position to be easily pulled laterally, resulting in adhesive deficiency, cracking and other undesirable phenomena at the bending position of the product.
[0003] Therefore, it is necessary to provide a new technical solution to solve the above technical problems. Summary of the invention
[0004] An object of the present invention is to provide a method for preparing a composite material, a composite material and a new technical solution for electronic equipment.
[0005] According to a first aspect of the present invention, a method for preparing a composite material is provided. The method comprises: Provide contoured tooling that matches the mold core structure; Preforming the prepreg in a contoured tooling and hardening and shaping it to form a preform; The preform is placed in the mold core structure of the mold and subjected to compression molding.
[0006] Optionally, the prepreg includes a thermosetting material and a fiber material, the thermosetting material includes at least one of epoxy resin and phenolic resin, and the fiber material includes at least one of carbon fiber, glass fiber and aramid fiber.
[0007] Optionally, the prepreg includes a thermoplastic material and a fiber material, the thermoplastic material includes at least one of polypropylene, nylon, polycarbonate, and polyetheretherketone, and the fiber material includes at least one of carbon fiber, glass fiber, and aramid fiber.
[0008] Optionally, the profiling tooling comprises a concave die and a convex die, and the prepreg is located between the concave die and the convex die during preforming.
[0009] Optionally, the contoured tooling is made of metal or resin.
[0010] Optionally, the prepreg comprises a thermosetting material, and the contoured tooling is made of metal; or The prepreg comprises a thermoplastic material, and the material of the contoured tooling is a resin.
[0011] Optionally, the prepreg includes a thermosetting material, and after preforming, the prepreg is placed in a low-temperature environment for hardening and setting, the temperature of the low-temperature environment is -20°C-0°C, and the hardening and setting time is 30s-100s.
[0012] Optionally, in the step of placing the preform in the mold core structure of the mold and performing compression molding, The prepreg comprises a thermosetting material, and the preformed part is placed on the male mold core of the mold core structure and is compression molded.
[0013] Optionally, during compression molding, the temperature of the mold is 100°C-160°C, the vacuuming time is 100s-300s, and the molding pressure is 20 kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0014] Optionally, in the step of placing the preform in the mold core structure of the mold and performing compression molding, The prepreg comprises a thermoplastic material, and the preform is placed in the male mold core or the female mold core of the mold core structure and is compression molded.
[0015] Optionally, infrared heating is used for compression molding, the infrared heating temperature is 300℃-600℃, the infrared heating time is 10s-100s; the temperature of the mold is 40℃-200℃, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0016] Optionally, in the step of preforming the prepreg in the profiling tooling and hardening and shaping to form a preformed part, a hot air gun is used to heat and soften the prepreg, and the setting temperature of the hot air gun is 50° C.-100° C., and the heating time is 5s-15s.
[0017] According to a second aspect of the present invention, a composite material is provided. The composite material is prepared according to the composite material preparation method of the present invention.
[0018] Optionally, the composite material has a thickness of 0.2 mm-2 mm.
[0019] According to a third aspect of the present invention, an electronic device is provided, comprising the composite material of the present invention.
[0020] In the embodiment of the present invention, a prepreg with a complex structure is preformed by a profiling tool to form a preform, and then the preform with a set structure is compression molded in a mold. Preforming and compression molding can effectively avoid the occurrence of adhesive deficiency, cracking and other undesirable phenomena at the bending position during the one-time compression molding process, and significantly improve the yield rate of the composite material. In addition to complex bending structures, complex structures such as high depth and large curvature can also be achieved by the preparation method of the embodiment of the present invention.
[0021] In addition, the heating temperature of the prepreg during preforming is lower than that of the prepreg during compression molding, which makes the preparation method simple in process and easy to operate.
[0022] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0024] Figure 1 is a flow chart of a method for preparing a composite material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0025] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0026] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0027] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0028] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0029] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0030] According to one embodiment of the present invention, a method for preparing a composite material is provided. Figure 1As shown, the preparation method comprises: Provide contoured tooling that matches the mold core structure; Preforming the prepreg in a contoured tooling and hardening and shaping it to form a preform; The preform is placed in the mold core structure of the mold and subjected to compression molding.
[0031] In this embodiment, the mold core structure of the mold includes a male mold core and a female mold core. The male mold core and the female mold core match the structure of the product. During compression molding, the prepreg is clamped between the male mold core and the female mold core to form a product with a set structure. The profiling tool is used to preform the prepreg. The profiling tool has a male mold that matches the structure of the male mold core and a female mold that matches the structure of the female mold core.
[0032] During preforming, the prepreg is placed on a male or female mold and heated to soften, and then the mold is closed. During the closing process, the prepreg forms a set structure. The prepreg is cured by natural cooling or accelerated cooling to form a preform. It should be pointed out that the heating temperature of preforming is lower than the heating temperature of compression molding. It is only necessary to form the prepreg into structures such as bends, arcs, and bevels according to the structural design requirements of the product during preforming. During the preforming process, at the bending position, the resin of the prepreg remains stationary while the fibers are bent, and the resin will not move away from the original position, so that there will not be too little resin in some areas, avoiding problems such as lack of glue and cracking.
[0033] For further shaping, the preform is placed in the mold core structure of the mold for compression molding. During the compression molding process, the preform is fully heated, vacuumed, pressed, and maintained to finally form a product with a set structure. During the compression molding process, since the fiber has been bent during preforming, it will not continue to bend significantly, and the resin will not be pulled horizontally, and there will be no local lack of resin, thus effectively avoiding the lack of glue and cracking at the bending position.
[0034] In the embodiment of the present invention, a prepreg with a complex structure is preformed by a profiling tool to form a preform, and then the preform with a set structure is compression molded in a mold. Preforming and compression molding can effectively avoid the occurrence of adhesive deficiency, cracking and other undesirable phenomena at the bending position during the one-time compression molding process, and significantly improve the yield rate of the composite material. In addition to complex bending structures, complex structures such as high depth and large curvature can also be achieved by the preparation method of the embodiment of the present invention.
[0035] In addition, the heating temperature of the prepreg during preforming is lower than that of the prepreg during compression molding, which makes the preparation method simple in process and easy to operate.
[0036] In a specific embodiment of the present invention, the prepreg includes a thermosetting material and a fiber material, the thermosetting material includes at least one of epoxy resin and phenolic resin, and the fiber material includes at least one of carbon fiber, glass fiber and aramid fiber.
[0037] In this embodiment, the thermosetting material refers to a resin material that undergoes chemical changes after heating, gradually hardens into shape, and does not soften when heated again. Optionally, epoxy resin and phenolic resin are both thermosetting materials, and the above materials are widely available and low in cost. One or more of these materials can be selected to prepare prepregs. The fiber material is selected from at least one of carbon fiber, glass fiber, and aramid fiber. For example, the weaving method of the fiber material can be a single-layer, unidirectional weaving. The prepreg is suitable for preforming and compression molding, and has few defects in the preparation process of composite materials.
[0038] In a specific embodiment of the present invention, the prepreg includes a thermoplastic material and a fiber material, the thermoplastic material includes at least one of polypropylene, nylon, polycarbonate, and polyetheretherketone, and the fiber material includes at least one of carbon fiber, glass fiber, and aramid fiber.
[0039] In this embodiment, the thermoplastic material refers to a resin material that softens after heating and hardens after cooling. Optionally, polypropylene, nylon, polycarbonate, and polyetheretherketone are all thermoplastic materials, and one or more of them can be selected to prepare the prepreg. The fiber material is, for example, at least one of carbon fiber, glass fiber, and aramid fiber. The fiber material is woven into unidirectional tape, plain weave, twill or satin weave. The prepreg is suitable for preforming and compression molding, and has few defects in the composite material preparation process.
[0040] In a specific embodiment of the present invention, the profiling tooling comprises a concave mold and a convex mold, and the prepreg is located between the concave mold and the convex mold during preforming.
[0041] The male and female molds are set according to the structure of the product. During preforming, the prepreg can be placed on the male mold first; then, the prepreg is heated so that the prepreg covers the male mold; next, the female mold is combined with the male mold, and under the extrusion of the male and female molds, the prepreg forms a set structure; finally, it is hardened and shaped to form a preform.
[0042] Alternatively, during preforming, the prepreg is first placed on the die; then, the prepreg is heated so that the prepreg covers the die; next, the male and female dies are combined, and under the extrusion of the male and female dies, the prepreg forms a set structure; finally, it is hardened and shaped to form a preform.
[0043] In a specific embodiment of the present invention, the contoured tooling is made of metal or resin.
[0044] Metals include aluminum alloys, copper alloys, stainless steel, carbon steel, etc. Milling, plasma cutting, etc. can be used to form concave molds, convex molds, etc. Metal materials have good heat dissipation effects, which are beneficial to the heating and cooling of prepregs. Resins include epoxy resins, phenolic resins, etc., which are cast to form concave molds, convex molds, etc. Resins have good thermal insulation effects, which are beneficial to the molding of prepregs.
[0045] In a specific embodiment of the present invention, the prepreg comprises a thermosetting material, and the material of the contoured tooling is metal.
[0046] In this embodiment, the material of the profiling tool is aluminum alloy. The profiling tool made of aluminum alloy is conducive to faster heat dissipation of the prepreg containing thermosetting material, thereby achieving hardening and shaping of the preform, avoiding irreversible curing of the prepreg due to overheating, and thus not affecting subsequent compression molding.
[0047] For example, during preparation, a prepreg slightly larger than the product is selected and placed on the concave mold of the profiling tooling. A hot air gun is used to evenly heat the prepreg until it softens. The softened prepreg is covered on the surface of the concave mold after the mold is closed. Since aluminum alloy materials dissipate heat quickly, the prepreg can be prevented from solidifying due to overheating.
[0048] Optionally, in the step of preforming the prepreg in the profiling tooling and hardening and shaping to form a preform, a hot air gun is used to heat and soften the prepreg, and the setting temperature of the hot air gun is 50°C-100°C, and the heating time is 5s-15s. If the setting temperature of the hot air gun is too low, and / or the heating time is too short, the prepreg is not easy to soften; on the contrary, if the setting temperature of the hot air gun is too high, and / or the heating time is too long, it is easy to cause the prepreg to be damaged due to overheating. Within the above range, the heating speed of the hot air gun is fast, and the above heating parameters can make the prepreg softening speed moderate. Of course, the specific heating parameters depend on the thickness and resin type of the composite material prepreg. When the prepreg softens to a suitable degree, the profiling tooling convex mold and the concave mold are molded. It should be pointed out that the temperature at which the hot air gun is heated and softened should be lower than the heating temperature when the thermosetting material undergoes irreversible curing, so as to facilitate subsequent compression molding.
[0049] Of course, the material of the contour tooling can also be copper alloy, stainless steel, carbon steel, etc.
[0050] In a specific embodiment of the present invention, the prepreg comprises a thermoplastic material, and the material of the contoured tooling is a resin.
[0051] In this embodiment, the profiling tool is made of epoxy resin. Since epoxy resin has good heat preservation effect, the profiling tool can slow down the rapid heat dissipation of the prepreg containing thermoplastic material, thereby helping to keep the prepreg softened and facilitating the preforming of the thermoplastic material.
[0052] For example, during preparation, a prepreg slightly larger than the product is selected and placed on the concave mold of the profiling tooling. A hot air gun is used to evenly heat the prepreg until it softens. The softened prepreg can cover the surface of the concave mold after the mold is closed. Since the epoxy resin dissipates heat slowly, the prepreg can effectively fill the gap between the concave mold and the convex mold.
[0053] For example, the set temperature of the hot air gun is 50℃-100℃, and the heating time is 5-15s. If the set temperature of the hot air gun is too low, and / or the heating time is too short, the prepreg is not easy to soften; on the contrary, if the set temperature of the hot air gun is too high, and / or the heating time is too long, the prepreg is easily damaged due to overheating. Within the above range, the softening speed of the prepreg can be moderate. Of course, the specific heating parameters depend on the thickness and resin type of the composite material prepreg. When the prepreg softens to an appropriate degree, the male and female molds of the profiling tooling are closed.
[0054] Of course, the material of the contoured tooling can also be phenolic resin.
[0055] In a specific embodiment of the present invention, the prepreg includes a thermosetting material. After preforming, the prepreg is placed in a low-temperature environment for hardening and shaping. The temperature of the low-temperature environment is -20°C to 0°C, and the hardening and shaping time is 30s-100s.
[0056] In this embodiment, in order to avoid irreversible curing of the thermosetting material due to long-term heating, the prepreg after preforming needs to be cured in a low-temperature environment. Optionally, the temperature of the low-temperature environment is -20°C to 0°C, and the curing and shaping time is 30s-100s. If the temperature of the low-temperature environment is too low, the requirements for the cooling equipment are high, and if the temperature of the low-temperature environment is too high, it is not conducive to the curing and shaping of the prepreg. Under the above conditions, the prepreg can be cured to form a preform, and the preform can still be heated and softened during the compression molding process to form a set structure.
[0057] Optionally, the temperature of the low temperature environment is -20°C, -18°C, -15°C, -12°C, -10°C, -8°C, -5°C, -3°C, 0°C. The curing and setting time is 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, etc. The above values can cure the prepreg to form a preform, and the preform can still be heated and softened during the compression molding process to form a set structure.
[0058] In a specific embodiment of the present invention, in the step of placing the preform in the core structure of the mold and performing compression molding, The prepreg comprises a thermosetting material, and the preformed part is placed on the male mold core of the mold core structure and is compression molded.
[0059] Before irreversible solidification occurs, the softening temperature of thermosetting materials is low. During the compression molding process, if the preform is placed on the female mold core of the mold core structure, the thermosetting material is easily softened by heat, thereby releasing stress, which will destroy the structure formed during the preforming process. In order to avoid the above phenomenon, during compression molding, the preform is placed on the male mold core of the mold core structure. In this way, even if the thermosetting material is softened by heat, the structure of the preform can maintain the structure formed during the preforming process due to the support of the male mold core, avoiding deformation of the preform caused by stress release.
[0060] In a specific embodiment of the present invention, during compression molding, the temperature of the mold is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0061] In this embodiment, the preform containing thermosetting material is taken out after cooling and setting, and placed on the male mold of the mold for hot pressing. The mold temperature is 100℃-160℃, the vacuum time is 100s-300s, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min. If the temperature of the mold is too low, the preform is not easy to soften; conversely, if the temperature of the mold is too high, the thermosetting material is easy to solidify. Within this temperature range, the preform softens, and the gas in the mold can be effectively discharged by vacuuming, so that the prepreg can fully fill the gap between the male core and the female core. If the molding pressure is too low, it is easy to cause the structure of the product to be loose and it is difficult to achieve the required thickness; if the molding pressure is too high, the requirements for the molding equipment are high. Under the above molding pressure, the prepreg reaches the set thickness and is easy to mold. Since the prepreg contains thermosetting material, under the above molding time, the thermosetting material undergoes a chemical reaction and solidifies and molds, and finally forms a product with a set structure.
[0062] Optionally, the temperature of the mold is 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, etc. The vacuuming time is 100s, 150s, 200s, 250s, 300s, etc. The molding pressure is 20kgf / cm 2 、60kgf / cm 2 、80kgf / cm 2 、100kgf / cm 2 、120kgf / cm 2 、140kgf / cm 2、160kgf / cm 2 、170kgf / cm 2 、180kgf / cm 2 The molding time is 0.5min, 1.0min, 1.5min, 2.0min, 2.5min, 3.0min, 3.5min, 4.0min, 4.5min, 5min, etc. The above values enable the prepreg to form a set structure and be cured.
[0063] In a specific embodiment of the present invention, in the step of placing the preform in the core structure of the mold and performing compression molding, The prepreg comprises a thermoplastic material, and the preform is placed in the male mold core or the female mold core of the mold core structure and is compression molded.
[0064] The softening temperature of thermoplastic materials is relatively high, for example, they need to reach the glass transition temperature of thermoplastic materials to soften, so at a lower temperature, the preform will not soften and deform. Therefore, before compression molding, placing the preform on the male or female mold core can maintain the structure formed during preforming. This makes the processing of prepregs containing thermoplastic materials easier.
[0065] In a specific embodiment of the present invention, infrared heating is used for compression molding, the infrared heating temperature is 300°C-600°C, the infrared heating time is 10s-100s; the temperature of the mold is 40°C-200°C, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
[0066] In this embodiment, infrared heating is used for compression molding. Infrared heating can directly heat the prepreg position without heating the mold itself, that is, the mold can maintain a low temperature, so that after the compression molding is completed, the prepreg can be quickly cooled down to harden the product, thereby reducing the time for heat dissipation of the product. The infrared heating method is particularly suitable for thermoplastic materials, which can quickly harden after the thermoplastic material is compression molded, thereby forming. If the compression molding is performed by directly heating the mold, the time required for the thermoplastic material to harden after compression molding is long because the mold cooling takes a long time. If the infrared heating temperature is too high and / or the heating time is too long, the prepreg is easily damaged; conversely, if the infrared heating temperature is too low and / or the heating time is too short, the prepreg is not easy to soften. The infrared heating temperature is 300℃-600℃, and the infrared heating time is 10s-100s. Within this range, the preform can be softened and the prepreg damage caused by the high temperature of the preform can be avoided. The temperature of the mold is 40℃-200℃. Within this range, after the infrared heating is completed, the preform can be cooled quickly to maintain the set structure. The molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min. Within the above range, under the above molding pressure and molding time, the prepreg can reach the set thickness and keep the thickness of each part uniform.
[0067] Optionally, the infrared heating temperature is 300°C, 400°C, 500°C, 600°C, etc., and the infrared heating time is 10s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, etc. The temperature of the mold is 40°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc. The molding pressure is 20kgf / cm 2 、40kgf / cm 2 、60kgf / cm 2 、80kgf / cm 2 、100kgf / cm 2 、120kgf / cm 2 、140kgf / cm 2 、160kgf / cm 2 、180kgf / cm 2 The molding time is 0.5min, 1.0min, 1.5min, 2.0min, 2.5min, 3.0min, 3.5min, 4.0min, 4.5min, 5min, etc. The above values can form the product into the set structure and reduce the processing time.
[0068] According to another embodiment of the present invention, a composite material is provided, which is prepared according to the composite material preparation method of the present invention.
[0069] The composite material has the characteristics of high molding precision, stable structure and high yield rate.
[0070] In a specific embodiment of the present invention, the thickness of the composite material is 0.2mm-2mm. For example, the thickness of the composite material is 0.2mm, 0.4mm, 0.6mm, 0.8mm, 1.0mm, 1.2mm, 1.4mm, 1.6mm, 1.8mm, 2mm, etc. The above thicknesses meet the requirements of thin and light electronic devices. In addition, the composite material has a good appearance without adhesive deficiency, cracking, or other undesirable appearance phenomena.
[0071] According to another embodiment of the present invention, an electronic device is provided, which includes the composite material of the present invention.
[0072] Optionally, the electronic device is a computer, a mobile phone, a watch, a television, a speaker, an AR device, a VR device, etc. For example, the composite material is used to prepare a housing of an electronic device. The electronic device of the present invention also includes at least all the beneficial effects of the above embodiments.
[0073] The following is a detailed description of the composite material preparation method and the composite material according to the embodiment of the present invention in combination with specific embodiments and comparative examples. It is worth noting that the following description is only exemplary and not a specific limitation to the present invention.
[0074] Example 1 The prepreg includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.5mm, and the layers are laid according to the fiber directions of 0°, 90°, 90°, and 0°. The thermosetting material is epoxy resin. The prepreg obtained by laying is placed on the concave mold of the profiling tooling made of aluminum alloy, and is evenly heated with a hot air gun until it softens. The set temperature of the hot air gun is 70°C, and the heating time is 10s. After the heating is completed, the male mold and the female mold of the profiling tooling are molded together. The profiling tooling is placed in a freezer as a whole for low-temperature cooling at a temperature of -18°C and a placement time of 50s. Next, take out the profiling tooling and take out the preform. The cooled and shaped preform is quickly placed on the male mold core of the hot pressing mold to ensure that the structure of the preform is basically the same as that of the male mold core, and compression molding is performed. The temperature of the mold is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 The molding time is 3 minutes. Finally, a product with a set structure is obtained.
[0075] Example 2 The prepreg includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.5mm, and the layers are laid according to the fiber directions of 0°, 45°, 45°, and 0°. The thermosetting material is epoxy resin. The prepreg obtained by laying is placed on the concave mold of the profiling tooling made of aluminum alloy, and is evenly heated with a hot air gun until it softens. The set temperature of the hot air gun is 70°C, and the heating time is 10s. After the heating is completed, the male mold and the female mold of the profiling tooling are molded together. The profiling tooling is placed in a freezer as a whole for low-temperature cooling at a temperature of -18°C and a placement time of 50s. Next, take out the profiling tooling and take out the preform. The cooled and shaped preform is quickly placed on the male mold core of the hot pressing mold to ensure that the structure of the preform is basically the same as that of the male mold core, and compression molding is performed. The temperature of the mold is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 The molding time is 3 minutes. Finally, a product with a set structure is obtained.
[0076] Example 3 The prepreg includes carbon fiber and thermoplastic material, wherein the diameter of the carbon fiber is 0.5mm and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate. The prepreg obtained by plying is placed on the concave mold of the epoxy resin profiling tooling, and is evenly heated with a hot air gun until it softens. The set temperature of the hot air gun is 170°C, and the heating time is 30s. After the heating is completed, the male and female molds of the profiling tooling are closed. The profiling tooling is cooled naturally. Next, take out the preform. The preform is quickly placed on the male mold core of the mold to ensure that the structure of the preform and the male mold core is basically the same, and compression molding is performed. The temperature of the mold is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, and the heating time is 1min. The compression molding pressure is 100kgf / cm 2 The molding time is 1 min. Finally, a product with a set structure is obtained.
[0077] Example 4 The prepreg includes glass fiber and thermoplastic material, wherein the diameter of the glass fiber is 0.5mm and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate. The prepreg obtained by plying is placed on the concave mold of the epoxy resin profiling tooling, and is evenly heated with a hot air gun until it softens. The set temperature of the hot air gun is 170°C, and the heating time is 30s. After the heating is completed, the male and female molds of the profiling tooling are closed. The profiling tooling is cooled naturally. Next, take out the preform. The preform is quickly placed on the male mold core of the mold to ensure that the structure of the preform and the male mold core is basically the same, and compression molding is performed. The temperature of the mold is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, and the heating time is 1min. The compression molding pressure is 100kgf / cm2 The molding time is 1 min. Finally, a product with a set structure is obtained.
[0078] Comparative Example 1 The prepreg includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.5mm, and the layers are laid in the fiber direction of 0°, 90°, 90°, and 0°. The thermosetting material is epoxy resin. The prepreg obtained by laying is placed on the concave mold of the mold for compression molding. The mold temperature is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 , the molding time is 3min.
[0079] Comparative Example 2 The prepreg includes carbon fiber and thermosetting material, wherein the diameter of the carbon fiber is 0.5mm, and the layers are laid in the fiber directions of 0°, 45°, 45°, and 0°. The thermosetting material is epoxy resin. The prepreg obtained by laying is placed on the concave mold of the mold for compression molding. The mold temperature is 130°C, the vacuum time is 150s, and the compression molding pressure is 30kgf / cm 2 , the molding time is 3min.
[0080] Comparative Example 3 The prepreg includes carbon fiber and thermoplastic material, wherein the diameter of the carbon fiber is 0.5 mm and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate. The prepreg is placed on the concave mold core of the mold, the temperature of the mold is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, the heating time is 1 minute, and compression molding is performed. The compression molding pressure is 100kgf / cm 2 ; The molding time is 1min.
[0081] Comparative Example 4 The prepreg includes glass fiber and thermoplastic material, wherein the diameter of the glass fiber is 0.5 mm and the fiber weaving method is plain weave. The thermoplastic material is transparent polycarbonate. The prepreg is placed on the concave mold core of the mold, the temperature of the mold is 90°C, and infrared heating is used for plasticization. The infrared heating temperature is 400°C, the heating time is 1 minute, and compression molding is performed. The compression molding pressure is 100kgf / cm 2 ; The molding time is 1min.
[0082] The product appearance results of the embodiments and comparative examples are shown in Table 1.
[0083] Table 1 - Comparison of product appearance of examples and comparative examples
[0084] As can be seen from Table 1, the composite material products prepared by the preparation method of the present invention in Examples 1-4 are bright in appearance, without adhesive deficiency, cracking and other undesirable appearance phenomena. However, the composite material products prepared by the preparation method of Comparative Examples 1-4 are rough in appearance, with adhesive deficiency and cracking at the bending position, which do not meet the appearance requirements. This shows that the embodiments of the present invention use contoured tooling to preform the prepreg of complex structure to form a preformed part, and then the preformed part with a set structure is compression molded in a mold. Preforming and compression molding can effectively avoid the occurrence of undesirable phenomena such as adhesive deficiency and cracking at the bending position during a single compression molding process, and significantly improve the yield rate of the composite material. In addition, the heating temperature of the prepreg during preforming is lower than the heating temperature of the prepreg during compression molding, which makes the preparation method simple in process and easy to operate.
[0085] Take the composite material prepared by the preparation method of Example 2 and Comparative Example 2 as an example. The preparation method of Example 2 uses a contouring tool to preform the prepreg of a complex structure to form a preform, and then the preform that has formed the set structure is compression molded in a mold. Preforming and compression molding can effectively avoid the occurrence of undesirable phenomena such as lack of glue and cracking at the bending position during a single compression molding process. Therefore, at the bend, the composite material of Example 2 is complete and transparent, which indicates that the structure of the composite material is complete and there is no cracking or lack of glue. At the bend, the composite material of Comparative Example 2 has exposed carbon filaments. This is because the epoxy resin is subjected to excessive tension during molding at this location and cannot be leveled to cover the surface of the product at the bend, resulting in lack of glue, so that the carbon fiber is exposed due to lack of glue, and the carbon fiber cannot be attached to the mold surface and cracks occur, resulting in appearance defects at the bend of the product.
[0086] The above embodiments focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0087] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A method for preparing a composite material, It is characterized in that include: Provide contoured tooling that matches the mold core structure; Preforming the prepreg in a contoured tooling and hardening and shaping it to form a preform; The preform is placed in the mold core structure of the mold and subjected to compression molding.
2. The method for preparing a composite material according to claim 1, It is characterized in that The prepreg includes a thermosetting material and a fiber material. The thermosetting material includes at least one of epoxy resin and phenolic resin. The fiber material includes at least one of carbon fiber, glass fiber and aramid fiber.
3. The method for preparing a composite material according to claim 1, It is characterized in that The prepreg comprises a thermoplastic material and a fiber material, wherein the thermoplastic material comprises at least one of polypropylene, nylon, polycarbonate, and polyetheretherketone, and the fiber material comprises at least one of carbon fiber, glass fiber, and aramid fiber.
4. The method for preparing a composite material according to claim 1, It is characterized in that The profiling tooling comprises a concave die and a convex die, and the prepreg is located between the concave die and the convex die during preforming.
5. The method for preparing a composite material according to claim 1, It is characterized in that The material of the contour tooling is metal or resin.
6. The method for preparing a composite material according to claim 1, It is characterized in that The prepreg comprises a thermosetting material, and the material of the contoured tooling is metal; or The prepreg comprises a thermoplastic material, and the material of the contoured tooling is a resin.
7. The method for preparing a composite material according to claim 1, It is characterized in that The prepreg includes a thermosetting material. After preforming, the prepreg is placed in a low-temperature environment for hardening and shaping. The temperature of the low-temperature environment is -20°C-0°C, and the hardening and shaping time is 30s-100s.
8. The method for preparing a composite material according to claim 1, It is characterized in that In the step of placing the preform in the mold core structure of the mold and performing compression molding, The prepreg comprises a thermosetting material, and the preformed part is placed on the male mold core of the mold core structure and is compression molded.
9. The method for preparing a composite material according to claim 8, It is characterized in that During compression molding, the temperature of the mold is 100°C-160°C, the vacuum time is 100s-300s, and the molding pressure is 20 kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
10. The method for preparing a composite material according to claim 1, It is characterized in that In the step of placing the preform in the mold core structure of the mold and performing compression molding, The prepreg comprises a thermoplastic material, and the preform is placed in the male mold core or the female mold core of the mold core structure and is compression molded.
11. The method for preparing a composite material according to claim 10, It is characterized in that Infrared heating is used for compression molding, the infrared heating temperature is 300℃-600℃, the infrared heating time is 10s-100s; the temperature of the mold is 40℃-200℃, and the molding pressure is 20kgf / cm 2 -180kgf / cm 2 , the molding time is 0.5min-5min.
12. The method for preparing a composite material according to claim 1, It is characterized in that In the step of preforming the prepreg in the profiling tooling and hardening and shaping to form the preformed part, a hot air gun is used to heat and soften the prepreg, the setting temperature of the hot air gun is 50° C.-100° C., and the heating time is 5s-15s.
13. A composite material, It is characterized in that The composite material is prepared according to the method for preparing the composite material according to any one of claims 1 to 12.
14. The composite material according to claim 13, It is characterized in that The thickness of the composite material is 0.2 mm-2 mm.
15. An electronic device, It is characterized in that Comprising the composite material as claimed in claim 13 or 14.
Citation Information
Patent Citations
Forming method of carbon fiber helmet shell and helmet
CN117644669A
Methods for composite material processing
GB201310930D0