Titanium steel composite plate with FeCoNiCr series high-entropy alloy as transition layer and preparation method of titanium steel composite plate
By using a FeCoNiCr-based high-entropy alloy transition layer in titanium-steel composite plates and optimizing the rolling process, the problems of insufficient interfacial bonding strength and corrosion resistance in titanium-steel composite plates have been solved, enabling the preparation of large-size high-end composite plates suitable for marine engineering and other fields.
Patent Information
- Application Number
- CN202410820924.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Existing titanium-steel composite plates are prone to generating brittle intermetallic compounds during the rolling process, resulting in insufficient interfacial bonding strength, and the transition layer material fails to effectively improve the corrosion resistance of the composite plate.
Using FeCoNiCr series high-entropy alloys as transition layers, and through reasonable billet assembly and rolling temperature control, the rolling process is optimized to control the diffusion of alloying elements and the formation of intermetallic compounds at the interface, thereby achieving high-quality rolling composite of steel and titanium.
The interfacial bonding performance and corrosion resistance of titanium-steel composite plates have been improved, enabling the production of large-size high-end titanium-steel composite plates suitable for marine engineering and other fields.
Smart Images

Figure CN118906581A_ABST
Abstract
Description
[Technical field]
[0001] The invention relates to the technical field of titanium steel composite plate preparation, and in particular to a titanium steel composite plate with a FeCoNiCr series high entropy alloy as a transition layer and a preparation method thereof. [Background technology]
[0002] Steel has good mechanical properties and machinability, and its cost is relatively low, but its corrosion resistance is average; titanium has high specific strength and excellent corrosion resistance, but its cost is high, especially when used as a structural component, the economic issue is worth considering. Titanium / steel composite combines steel and titanium in a reasonable way, which not only obtains the performance advantages of the two materials, but also reduces the cost of components. It has gradually become a substitute for single titanium and is widely used in civil and defense industries such as petroleum, chemical industry and marine engineering. The preparation methods of titanium steel composite plates mainly include: explosion composite method, diffusion composite method, explosion composite-rolling method and rolling composite method. However, the process of the explosion composite method is relatively complicated, and the energy consumption is large, the environment is polluted, and the yield rate is relatively low. The size of the composite plate produced by the diffusion composite method is small, which is difficult to meet the user's requirements for the use of large-size plates. Due to the continuous iteration and upgrading of large-tonnage rolling mills and the continuous progress of rolling technology for large-size composite plates, large-size titanium steel composite plates can now be produced by rolling, which will greatly reduce the cost of titanium steel composite plates.
[0003] However, there are large differences in chemical composition and physical properties (such as melting point, linear expansion coefficient, thermal conductivity and specific heat capacity) between titanium and steel, which leads to the formation of brittle intermetallic compounds and titanium carbide phases when the two are compounded, thereby reducing the bonding strength of the interface. Therefore, when titanium steel is rolled and compounded, the formation of interfacial brittle phases is usually reduced by adding a transition layer metal between titanium and steel, thereby improving the interfacial bonding strength. CN104907333A discloses a method for preparing a titanium-steel composite plate with nickel as an intermediate layer, CN104998903A discloses a method for preparing a titanium-steel composite plate with copper as an intermediate layer, and CN109693433B discloses a method for preparing a titanium-steel composite plate with IF steel as an intermediate layer. The addition of the transition layer metal effectively prevents the mutual diffusion between titanium and iron and improves the bonding effect of the composite interface.
[0004] Studies have shown that high entropy alloys (HEA) have four typical effects: high entropy effect in thermodynamics, hysteresis diffusion effect in kinetics, lattice distortion effect in structure, and cocktail effect in performance. The specific manifestation of the high entropy effect is that a simple disordered solid solution structure is obtained after uniform mutual dissolution rather than an intermetallic compound; the hysteresis diffusion effect is reflected in the complexity of the chemical composition and the severity of the lattice distortion, which makes the diffusion of atoms in the alloy extremely difficult. These two effects will help prevent the formation of a thick intermetallic compound reaction layer at the interface during the connection of dissimilar metals, and greatly reduce the tendency of brittle failure during interface bonding. At the same time, unlike pure component transition layer metals, high entropy alloys (containing Cr) with corrosion resistance can improve the corrosion resistance of transition layers and composite plates. The FeCoNiCr series high entropy alloy is a candidate component system that can meet this requirement.
[0005] Therefore, in order to further improve the comprehensive interface performance of the titanium-steel composite plate, it is necessary to develop a titanium-steel composite plate with high corrosion resistance and excellent interface bonding performance and a preparation method thereof. Therefore, the present invention provides a titanium-steel composite plate with a FeCoNiCr-based high-entropy alloy as a transition layer and a preparation method thereof to address the shortcomings of the prior art and to solve or alleviate one or more of the above-mentioned problems. [Summary of the invention]
[0006] In view of this, the present invention provides a titanium-steel composite plate with a FeCoNiCr-based high-entropy alloy as a transition layer and a preparation method thereof, which realizes high-quality rolling composite of steel and titanium by reasonable blanking and rolling temperature control, optimizing the rolling process, controlling the diffusion of alloy elements at the interface and the formation of intermetallic compounds.
[0007] On the one hand, the present invention provides a titanium-steel composite plate with a FeCoNiCr-based high-entropy alloy as a transition layer, wherein the titanium-steel composite plate includes a steel layer and a titanium layer, and the titanium-steel composite plate also includes a transition layer, wherein the steel layer is connected to the titanium layer through the transition layer, and the transition layer is a FeCoNiCr-based high-entropy alloy.
[0008] According to the aspects described above and any possible implementation method, an implementation method is further provided, wherein the composition range of each component of the FeCoNiCr high-entropy alloy is greater than 5.0wt.% and less than 35.0wt.%, wherein 5.0%≤Fe≤35.0%, 5.0%≤Co≤35.0%, 5.0%≤Ni≤35.0%, and 5.0%≤Cr≤35.0%.
[0009] According to the above aspects and any possible implementation, an implementation is further provided, wherein the steel layer is a plain carbon steel plate, and the plain carbon steel plate is one or more of Q235 or Q345.
[0010] According to the above aspects and any possible implementation, an implementation is further provided, wherein the titanium material layer is an industrial titanium plate, and the industrial titanium plate is one or more of TA1 or TA2.
[0011] According to the above aspects and any possible implementation, an implementation is further provided, wherein the length ratio and width ratio of the steel layer and the titanium layer are both 1, and the thickness ratio is 1.0 to 5.0.
[0012] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the length and width of the transition layer are the same as those of the steel layer and / or the titanium layer, and the thickness is 0.5 to 1.0 mm;
[0013] The steel layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 10 to 30 mm;
[0014] The titanium material layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 5 to 20 mm.
[0015] According to the aspects described above and any possible implementation method, an implementation method is further provided, wherein the titanium-steel composite plate also includes a coating layer and an isolation layer, the coating layer includes an upper plate layer, a lower plate layer and four peripheral side plate layers, the upper plate layer is connected to the steel layer through the isolation layer, the lower plate layer is connected to the titanium layer through the isolation layer, and the four peripheral side plate layers are respectively coated on the four peripheral sides of the upper and lower connected steel layer and titanium layer.
[0016] According to the aspects described above and any possible implementation method, an implementation method is further provided, wherein the coating layer is ordinary carbon steel A3, the length and width of the upper plate layer and the lower plate layer are 20 mm more than the steel layer, and the thickness of the upper plate layer and the lower plate layer are both 6 to 10 mm.
[0017] According to the above aspects and any possible implementation, an implementation is further provided, wherein the isolation layer is a glass fiber isolation cloth, the length and width of the isolation layer are the same as those of the steel layer, and the thickness of the isolation layer is 1 to 2 mm.
[0018] According to the above aspects and any possible implementation, a method for preparing a titanium-steel composite plate with a FeCoNiCr-based high entropy alloy as a transition layer is further provided, the preparation method comprising the following steps:
[0019] S1: Preset the coating layer, isolation layer, steel layer, transition layer and titanium layer, wherein the coating layer is arranged outside the steel layer and the titanium layer, the isolation layer is arranged between the steel layer and the coating layer and between the titanium layer and the coating layer, and the transition layer is arranged for quality inspection of the steel layer and the titanium layer;
[0020] S2: Select ordinary carbon steel plate as the raw material for the steel layer, select industrial titanium plate as the raw material for the titanium layer; select high entropy alloy thin plate as the raw material for the transition layer;
[0021] S3: Ordinary carbon steel A3 is selected as the cladding layer, and glass fiber isolation cloth is selected as the isolation layer;
[0022] S4: pre-treating the surfaces of the steel layer and the titanium layer to be in contact;
[0023] S5: assembling the composite plate in a preset manner;
[0024] S6: The gaps between the cladding layer and the steel layer and the titanium layer are completely filled with ordinary carbon steel A3, and a circular hole with a diameter of 5 to 10 mm is reserved on either side of the cladding layer to form a first composite blank;
[0025] S7: Perform multiple passes of argon arc welding on the four sides of the first composite billet, with a weld depth of 15 to 20 mm. After welding, perform vacuum treatment through the reserved holes, with a vacuum degree of less than 5×10 -2 Pa, forming a second composite blank;
[0026] S8: heating the second composite billet to 890±20°C for 2-4h, starting rolling at 845±20°C, reducing by 15%-30% per pass, with a total reducing by ≥75%, finishing at 720°C or above, and air cooling to room temperature to form a third composite billet;
[0027] S9: trimming, removing the sheath, and grinding the surface of the third composite blank to obtain a titanium-steel composite plate with a thickness of 2 to 16 mm. The plate width can reach 2.5 to 3 m, and the thickness ratio of the titanium-steel layer is adjustable.
[0028] Compared with the prior art, the present invention can achieve the following technical effects:
[0029] The rolling process of the present invention is simple, and the requirements for the raw material plate are relatively low. The width of the composite plate finally prepared can reach 2.5 to 3 meters, and the thickness ratio of the titanium steel layer is adjustable. The transition layer high entropy alloy has anti-corrosion properties and can be used in marine engineering, outdoor and other fields, which can greatly increase the development and promotion of high-end titanium steel composite products.
[0030] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time.
Brief Description of the Drawings
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 This is a method for assembling a composite plate containing a transition layer provided by an embodiment of the present invention;
[0033] Among them, in the figure:
[0034] 1-Outer sheath is ordinary carbon steel A3, 2-glass fiber isolation cloth, 3-ordinary carbon steel (Q235 or Q345), 4-high entropy alloy transition layer, 5-titanium material (TA1 or TA2). [Specific implementation method]
[0035] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0036] It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0038] The present invention provides a titanium-steel composite plate with a FeCoNiCr series high entropy alloy as a transition layer and a preparation method thereof, wherein the titanium-steel composite plate is composed of a coating layer, an isolation layer, a steel layer, a transition layer and a titanium layer, wherein:
[0039] The steel layer and the titanium layer are connected up and down through the transition layer;
[0040] The coating layer includes an upper plate layer, a lower plate layer and four peripheral side plate layers. The upper plate layer is connected to the steel layer through an isolation layer, the lower plate layer is connected to the titanium layer through an isolation layer, and the four peripheral side plate layers are respectively coated on the four peripheral sides of the upper and lower connected steel layer and titanium layer.
[0041] The length ratio and width ratio of the steel layer and the titanium layer are both 1, and the thickness ratio is 1.0-5.0. The raw material for the steel layer is ordinary carbon steel plate, and the raw material for the titanium layer is industrial titanium plate. The transition layer has the same length and width as the steel layer, and a thickness of 0.5-1.0 mm.
[0042] The plain carbon steel plate is one or more of Q235 and Q345.
[0043] The industrial titanium plate is one or more of TA1 or TA2.
[0044] The steel layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 10 to 30 mm.
[0045] The titanium material layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 5 to 20 mm.
[0046] The transition layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 0.5 to 1.0 mm.
[0047] The cladding layer is ordinary carbon steel A3, the length and width of the upper plate layer and the lower plate layer are 20 mm greater than the steel layer, and the thickness of the upper plate layer and the lower plate layer are both 6 to 10 mm.
[0048] The isolation layer is a glass fiber isolation cloth. The length and width of the isolation layer are the same as those of the steel layer. The thickness of the isolation layer is 1 to 2 mm.
[0049] The present invention also provides a method for preparing a titanium-steel composite plate using a FeCoNiCr-based high entropy alloy as a transition layer, which is used to prepare the titanium-steel composite plate. The preparation method comprises the following steps:
[0050] S1: Preset the coating layer, isolation layer, steel layer, transition layer and titanium layer, wherein the coating layer is arranged outside the steel layer and the titanium layer, the isolation layer is arranged between the steel layer and the coating layer and between the titanium layer and the coating layer, and the transition layer is arranged for quality inspection of the steel layer and the titanium layer;
[0051] S2: Select ordinary carbon steel plate as the raw material for the steel layer, select industrial titanium plate as the raw material for the titanium layer; select high entropy alloy thin plate as the raw material for the transition layer;
[0052] S3: Ordinary carbon steel A3 is selected as the cladding layer, and glass fiber isolation cloth is selected as the isolation layer;
[0053] S4: pre-treating the surfaces of the steel layer and the titanium layer to be in contact;
[0054] S5: assembling the composite plate in a preset manner;
[0055] S6: The gaps between the cladding layer and the steel layer and the titanium layer are completely filled with ordinary carbon steel A3, and a circular hole with a diameter of 5 to 10 mm is reserved on either side of the cladding layer to form a first composite blank;
[0056] S7: Perform multiple passes of argon arc welding on the four sides of the first composite billet, with a weld depth of 15 to 20 mm. After welding, perform vacuum treatment through the reserved holes, with a vacuum degree of less than 5×10 -2 Pa, forming a second composite blank;
[0057] S8: heating the second composite billet to 890±20°C for 2-4h, starting rolling at 845±20°C, reducing by 15%-30% per pass, with a total reducing by ≥75%, finishing at 720°C or above, and air cooling to room temperature to form a third composite billet;
[0058] S9: trimming, removing the sheath, and grinding the surface of the third composite blank to obtain a titanium-steel composite plate with a thickness of 2 to 16 mm. The plate width can reach 2.5 to 3 m, and the thickness ratio of the titanium-steel layer is adjustable.
[0059] The preprocessing process in S4 includes:
[0060] S41: machining the surfaces of the steel layer and the titanium layer to be in contact by a grinder to remove scales and stains on the surfaces to be in contact;
[0061] S42: Use alcohol solvent to deeply clean the surface of the machined steel layer and titanium layer and blow dry the workpiece surface.
[0062] Embodiment 1:
[0063] Steel: Q235 (mass percentage by wt.%, C≤0.20%, Si≤0.30%, Mn≤0.70%, P≤0.045%, S≤0.045%, balance Fe), size: 200×1000×25mm.
[0064] High entropy alloy: HEA1 (mass percentage wt.%, Fe: 24.0-26.0%, Co: 24.0-26.0%, Ni: 24.0-26.0%, Cr: 24.0-26.0%), size: 200×1000×0.75mm.
[0065] Titanium material: pure titanium TA1 (mass percentage wt.%, H≤0.015%, O≤0.20%, Fe≤0.25%, C≤0.10%, N≤0.03%, the remainder is Ti), size: 200×1000×10mm.
[0066] The specific steps are as follows:
[0067] S1: Use a grinder to machine the contact surfaces of steel and titanium to remove scale and stains on the contact surfaces; use alcohol solvent to deeply clean the processed steel and titanium surfaces and blow dry the workpiece surface.
[0068] S2: The materials and methods of assembly are ordinary carbon steel A3, glass fiber isolation cloth, ordinary carbon steel Q235, high entropy alloy HEA transition layer metal, TA1 titanium material, glass fiber isolation cloth, and ordinary carbon steel A3.
[0069] S3: The space between two ordinary carbon steel A3 is completely filled with the same material, and a circular hole with a diameter of 5 to 10 mm is left on one side for welding and sealing after vacuuming to form a composite billet; the four sides of the composite billet are subjected to multi-pass argon arc welding, and the weld depth is 15 to 20 mm. After welding, vacuum treatment is performed through the reserved hole, and the vacuum degree is less than 5.0×10 -2 Pa.
[0070] S4: heating the composite billet after welding to 890±20℃ and keeping it warm for 2h, the starting rolling temperature is 845±20℃, the single pass reduction rate is 25%, the total reduction rate is ≥70%, the final rolling temperature is above 720℃, and air cooling is performed to room temperature.
[0071] S5: After the rolled composite plate is trimmed, the jacket is removed, and the surface is ground, a high-strength titanium-steel composite plate with a thickness of 8 mm is obtained, the plate width can reach 3.2 m, and the titanium-steel layer thickness ratio is 0.4.
[0072] According to mechanical properties testing, the shear strength of the titanium-steel composite interface containing high-entropy alloy transition layer metal is 299MPa.
[0073] Embodiment 2:
[0074] Steel: Q345 (mass percentage by wt.%, C≤0.20%, Si≤0.55%, Mn≤1.60%, P≤0.045%, S≤0.045%, balance Fe), size: 200×1000×20mm.
[0075] High entropy alloy: HEA2 (mass percentage wt.%, Fe: 29.0-31.0%, Co: 19.0-21.0%, Ni: 24.0-26.0%, Cr: 24.0-26.0%), size: 200×1000×0.90mm.
[0076] Titanium material: pure titanium TA1 (mass percentage wt.%, H≤0.015%, O≤0.20%, Fe≤0.25%, C≤0.10%, N≤0.03%, the remainder is Ti), size: 200×1000×10mm.
[0077] The specific steps are as follows:
[0078] S1: Use a grinder to machine the contact surfaces of steel and titanium to remove scale and stains on the contact surfaces; use alcohol solvent to deeply clean the processed steel and titanium surfaces and blow dry the workpiece surface.
[0079] S2: The materials and methods of assembly are ordinary carbon steel A3, glass fiber isolation cloth, ordinary carbon steel Q235, high entropy alloy HEA transition layer metal, TA1 titanium material, glass fiber isolation cloth, and ordinary carbon steel A3.
[0080] S3: The space between two ordinary carbon steel A3 is completely filled with the same material, and a circular hole with a diameter of 5 to 10 mm is left on one side for welding and sealing after vacuuming to form a composite billet; the four sides of the composite billet are subjected to multi-pass argon arc welding, and the weld depth is 15 to 20 mm. After welding, vacuum treatment is performed through the reserved hole, and the vacuum degree is less than 5.0×10 -2 Pa.
[0081] S4: heating the composite billet after welding to 890±20℃ and keeping it warm for 2h, the starting rolling temperature is 845±20℃, the single pass reduction rate is 25%, the total reduction rate is ≥70%, the final rolling temperature is above 720℃, and air cooling is performed to room temperature.
[0082] S5: After the rolled composite plate is trimmed, the jacket is removed, and the surface is ground, a high-strength titanium-steel composite plate with a thickness of 8 mm is obtained, the plate width can reach 3.2 m, and the titanium-steel layer thickness ratio is 0.5.
[0083] According to mechanical properties testing, the shear strength of the titanium-steel composite interface containing high-entropy alloy transition layer metal is 344MPa.
[0084] The above is a detailed introduction to a titanium steel composite plate with a FeCoNiCr high entropy alloy as a transition layer and a preparation method thereof provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and its core idea of the present application; at the same time, for a person skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
[0085] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.
[0086] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0087] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0088] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A titanium-steel composite plate with a FeCoNiCr-based high entropy alloy as a transition layer, the titanium-steel composite plate comprising a steel layer and a titanium layer, characterized in that: The titanium-steel composite plate further includes a transition layer, the steel layer is connected to the titanium layer via the transition layer, and the transition layer is a FeCoNiCr series high entropy alloy.
2. The titanium steel composite plate according to claim 1, characterized in that: The composition range of each component of the FeCoNiCr high entropy alloy is greater than 5.0wt.% and less than 35.0wt.%, wherein 5.0%≤Fe≤35.0%, 5.0%≤Co≤35.0%, 5.0%≤Ni≤35.0%, and 5.0%≤Cr≤35.0%.
3. The titanium steel composite plate according to claim 1, characterized in that: The steel layer is a plain carbon steel plate, and the plain carbon steel plate is one or more of Q235 and Q345.
4. The titanium steel composite plate according to claim 1, characterized in that: The titanium material layer is an industrial titanium plate, and the industrial titanium plate is one or more of TA1 or TA2.
5. The titanium steel composite plate according to claim 1, characterized in that: The length ratio and width ratio of the steel material layer and the titanium material layer are both 1, and the thickness ratio is 1.0-5.
0.
6. The titanium steel composite plate according to claim 5, characterized in that: The length and width of the transition layer are the same as those of the steel layer and / or the titanium layer, and the thickness is 0.5 to 1.0 mm; The steel layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 10 to 30 mm; The titanium material layer has a length of 0.5 to 2 m, a width of 0.2 to 1 m, and a thickness of 5 to 20 mm.
7. The titanium steel composite plate according to claim 1, characterized in that: The titanium-steel composite plate also includes a coating layer and an isolation layer. The coating layer includes an upper plate layer, a lower plate layer and four peripheral side plate layers. The upper plate layer is connected to the steel layer through the isolation layer, and the lower plate layer is connected to the titanium layer through the isolation layer. The four peripheral side plate layers are respectively coated on the four peripheral sides of the upper and lower connected steel layer and titanium layer.
8. The titanium steel composite plate according to claim 7, characterized in that: The cladding layer is ordinary carbon steel A3, the length and width of the upper plate layer and the lower plate layer are 20 mm greater than the steel layer, and the thickness of the upper plate layer and the lower plate layer are both 6 to 10 mm.
9. The titanium steel composite plate according to claim 7, characterized in that: The isolation layer is a glass fiber isolation cloth. The length and width of the isolation layer are the same as those of the steel layer. The thickness of the isolation layer is 1 to 2 mm.
10. A method for preparing a titanium-steel composite plate with a FeCoNiCr series high entropy alloy as a transition layer, used for preparing the titanium-steel composite plate according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: S1: Preset the coating layer, isolation layer, steel layer, transition layer and titanium layer, wherein the coating layer is arranged outside the steel layer and the titanium layer, the isolation layer is arranged between the steel layer and the coating layer and between the titanium layer and the coating layer, and the transition layer is arranged for quality inspection of the steel layer and the titanium layer; S2: Select ordinary carbon steel plate as the raw material for the steel layer, select industrial titanium plate as the raw material for the titanium layer; select high entropy alloy thin plate as the raw material for the transition layer; S3: Ordinary carbon steel A3 is selected as the cladding layer, and glass fiber isolation cloth is selected as the isolation layer; S4: pre-treating the surfaces of the steel layer and the titanium layer to be in contact; S5: assembling the composite plate in a preset manner; S6: The gaps between the cladding layer and the steel layer and the titanium layer are completely filled with ordinary carbon steel A3, and a circular hole with a diameter of 5 to 10 mm is reserved on either side of the cladding layer to form a first composite blank; S7: Perform multiple passes of argon arc welding on the four sides of the first composite billet, with a weld depth of 15 to 20 mm. After welding, perform vacuum treatment through the reserved holes, with a vacuum degree of less than 5×10 -2 Pa, forming a second composite blank; S8: heating the second composite billet to 890±20°C for 2-4h, starting rolling at 845±20°C, reducing by 15%-30% per pass, with a total reducing by ≥75%, finishing at 720°C or above, and air cooling to room temperature to form a third composite billet; S9: trimming, removing the sheath, and grinding the surface of the third composite blank to obtain a titanium-steel composite plate with a thickness of 2 to 16 mm. The plate width can reach 2.5 to 3 m, and the thickness ratio of the titanium-steel layer is adjustable.
Citation Information
Patent Citations
Welding material and welding method for titanium-steel composite board
CN103567654A
Intermediate alloy for titanium / carbon steel bimetal compounding and compounding process
CN110936680A
Metal / high-entropy alloy laminated composite material and preparation method thereof
CN111497374A
Application of high-entropy alloy, titanium-steel bimetal composite plate and preparation method of titanium-steel bimetal composite plate
CN115740836A
Cited By
Preparation process of bimetal composite tee joint
CN121491348A