Flame-retardant high-strength high-impact polypropylene sheet and fabric thereof, flame-retardant polypropylene composite material and preparation method and application of flame-retardant high-strength high-impact polypropylene sheet
Through multi-layer structure and hot pressing technology, the problem of insufficient performance of flame-retardant polypropylene composite materials at low temperatures is solved, and the peel strength and impact performance between high-layers is improved, which broadens its application scenarios and is suitable for thin plates, films and fabrics. and other fields.
Patent Information
- Application Number
- CN202310506527.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-07
AI Technical Summary
It is difficult for existing flame-retardant polypropylene composite materials to have wide processing temperatures, strong mechanical properties, high interlayer peel strength and flame retardant properties at the same time, and their application scenarios are limited, especially not suitable for applications such as thin plates, films and fabrics.
Using multi-layer structure flame-retardant polypropylene sheets and fabrics, the flame-retardant polypropylene composite materials with excellent mechanical properties and high interlayer peel strength are prepared, with the differences between layers A and B. The difference in melting point and the reasonable proportion of flame retardant ensure that the material has good performance at lower heat pressing temperatures.
It realizes the high-layer peel strength and good impact performance of the flame-retardant polypropylene composite material at lower heat pressing temperatures, broadens its application scenarios, is suitable for thin plates, films and fabrics, and at the same time reduces equipment energy consumption and production cost.
Smart Images

Figure BDA0004216559220000201 
Figure BDA0004216559220000211
Abstract
Description
Technical Field
[0001] The invention relates to the field of polypropylene materials, and more particularly to a flame-retardant high-strength high-impact polypropylene sheet and fabric thereof, a flame-retardant polypropylene composite material, and a preparation method and application thereof. Background Art
[0002] Polypropylene (PP) resin has low density, good heat resistance, and good stiffness, hardness and weldability, which makes it widely used.
[0003] The matrix and reinforcing phase of self-reinforced polymer composites are composed of different forms of the same polymer, and the reinforcing phase is usually a highly oriented fiber or flat ribbon. Most self-reinforced polymer composites are prepared using a hot pressing method. When the reinforcing phase is hot pressed at a certain pressure and temperature, the surface of the reinforcing phase fiber melts to become a matrix melt. The matrix melt and the reinforcing phase surface co-crystallize when melted, thereby providing sufficient interfacial bonding strength. As in US6312638B1, melt-spun oriented polyolefin fibers are hot pressed, and a specific temperature and pressure are used to partially melt-bond the surface layer of the polyolefin to prepare a polyolefin sheet. This preparation method is not only sensitive to the temperature of hot pressing, but also has a high hot pressing temperature. In addition, the oriented fibers produce a large decomposition orientation after hot pressing, and the mechanical strength decreases significantly.
[0004] In order to widen the hot pressing window and reduce the hot pressing pressure, polyolefins with different melting points can be hot pressed. For example, US8133537B2 hot presses three layers of polyolefin fibers with different melting points to obtain a polyolefin composite material, wherein the melting temperatures of the first and second layers of polyolefins are lower than the core layer. However, the hot pressing composite material prepared by this method has low impact strength and interlayer peeling strength.
[0005] Polypropylene has poor flame retardancy and a low oxygen index of only 17.0-17.5%. It is a flammable material. When burning, it has a high heat release rate and high calorific value, and is very easy to spread flames and cause fires. These have greatly limited the use of polypropylene film products in industries such as electrical appliances, chemicals, machinery, and military products. Therefore, how to improve the flame retardancy of polymers has also attracted widespread attention.
[0006] At present, commonly used polypropylene flame retardants include halogen flame retardants, phosphorus-nitrogen flame retardants and inorganic flame retardants. Studies have shown that the addition of a large number of commercial flame retardants, while improving the flame retardant properties of the material, often destroys the comprehensive mechanical properties of the composite material, especially the impact performance, due to factors such as poor dispersion of the additive and the substrate, and there are technical difficulties in the contradiction between flame retardancy and mechanics. The existing technology usually uses a multi-component multifunctional (including flame retardants, toughening agents) system design to construct a high-impact flame-retardant composite material system. For example, Chinese invention patent CN103724806B discloses a high-impact flame-retardant polypropylene composite material for automotive functional parts and its preparation method, using acrylic rubber powder, polyolefin elastomer, polar monomer grafted polyolefin elastomer as a composite toughening agent, ensuring that the material has a UL94V-0 (1.6 mm) flame retardant rating while significantly improving the impact performance of the material. CN109776956A discloses a highly impact-resistant, highly rigid, flame-retardant and anti-drip polypropylene modified material, which is obtained by reasonably proportioning the flame retardant, reinforcing filler, surface-treated whisker, antioxidant, compatibilizer and other ingredients to obtain a modified material with good mechanical properties and flame retardant properties. The above-mentioned prior art maintains the mechanical properties of the flame-retardant polypropylene composite material from being seriously damaged by adding elastomers or reinforcing fillers, but the processing application scenarios of this method are limited and it is not suitable for thin plates, films, fabrics and the like.
[0007] In summary, how to provide a flame-retardant polypropylene composite material that has a wider processing temperature, stronger mechanical properties, higher interlaminar peel strength and flame retardant properties, and further broaden the application scenarios of flame-retardant polypropylene on the basis of maintaining the mechanical properties of the flame-retardant polypropylene composite material, so that it is suitable for applications such as thin plates, films, and fabrics, is a technical problem that needs to be solved at present. Summary of the invention
[0008] The purpose of the present invention is to overcome the technical defect that the existing flame-retardant polypropylene composite materials are difficult to have a wide processing temperature, strong mechanical properties, high interlayer peeling strength and flame retardant properties at the same time, and provide flame-retardant polypropylene sheets, flame-retardant polypropylene fabrics, high-strength and high-impact flame-retardant polypropylene composite materials and preparation methods and applications thereof. The flame-retardant polypropylene sheet of the present invention is subjected to hot pressing and the like to obtain a flame-retardant polypropylene composite material, and the flame-retardant polypropylene composite material has excellent mechanical properties and good interlayer peeling strength and flame retardant properties. Even at a lower hot pressing temperature and a wider hot pressing temperature range, the interlayer peeling strength of the obtained flame-retardant polypropylene composite material is still high; not only that, the flame-retardant polypropylene sheet, flame-retardant polypropylene fabric, and high-strength and high-impact flame-retardant polypropylene composite material of the present invention are also suitable for thin plates, films, and fabrics on the basis of maintaining the mechanical properties of the flame-retardant polypropylene composite material, thereby broadening the application scenarios of flame-retardant polypropylene.
[0009] In a first aspect, the present invention aims to provide a flame retardant polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB';
[0010] Wherein layer B and layer B' are the same or different, and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x, a thermal bonding enhancer y and an optional flame retardant n; layer A contains a polypropylene composition A, wherein the polypropylene composition A includes a homopolymer polypropylene a, an impact copolymer polypropylene b and an optional flame retardant m;
[0011] The melting point of the polypropylene composition A is greater than that of the polypropylene composition B and the polypropylene composition B', and the contents of the corresponding flame retardant m and flame retardant n in the polypropylene composition A, the polypropylene composition B and the polypropylene composition B' are not 0 at the same time.
[0012] According to the present invention, the film layers B and B' on both sides of the film layer A are the same or different. In a preferred embodiment of the present invention, the film layers B and B' on both sides of the film layer A are the same.
[0013] According to some preferred embodiments of the present invention, the melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10°C.
[0014] According to some preferred embodiments of the present invention, based on the total thickness of the flame retardant polypropylene sheet, the thickness of layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%. The thicknesses of the film layers B and B' on both sides of the film layer A can be the same or different, preferably the same.
[0015] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.
[0016] According to the present invention, the thickness of the film layers A, B, B' can be controlled by the melt pump of the extruder during the processing.
[0017] According to some preferred embodiments of the present invention, the difference between the melting points of polypropylene composition A and polypropylene composition B, and the difference between the melting points of polypropylene composition A and polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C.
[0018] According to some preferred embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 30-98wt% of homopolypropylene a, 1-50wt% of impact copolymer polypropylene b, and 0-60wt% of flame retardant m; preferably, the polypropylene composition A comprises 40-80wt% of homopolypropylene a, 5-30wt% of impact copolymer polypropylene b, and 2-50wt% of flame retardant m; more preferably, the polypropylene composition A comprises 40-80wt% of homopolypropylene a, 5-30wt% of impact copolymer polypropylene b, and 10-50wt% of flame retardant m.
[0019] More preferably, the polypropylene composition A comprises 40-80 wt% of homopolypropylene a, such as 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, and any two values or any interval between any two values.
[0020] More preferably, the polypropylene composition A comprises 5-30 wt% of the impact copolymer polypropylene b, such as 5 wt%, 10 wt%, 20 wt%, 30 wt%, and any two values or any interval between any two values.
[0021] More preferably, the polypropylene composition A comprises 10-50 wt% of the flame retardant m, for example 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, and any two values or any interval between any two values.
[0022] According to some preferred embodiments of the present invention, based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 30-98wt% of random copolymer polypropylene x, 1-50wt% of thermal adhesion enhancer y, and 0-60wt% of flame retardant n; preferably, the polypropylene composition B and the polypropylene composition B' each include 40-80wt% of random copolymer polypropylene x, 5-30wt% of thermal adhesion enhancer y, and 2-50wt% of flame retardant n; more preferably, the polypropylene composition B and the polypropylene composition B' each include 40-80wt% of random copolymer polypropylene x, 5-20wt% of thermal adhesion enhancer y, and 10-50wt% of flame retardant n.
[0023] More preferably, the polypropylene composition B and the polypropylene composition B' each comprise 40-80 wt% of the random copolymer polypropylene x, for example 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, and any two values or any interval between any two values.
[0024] More preferably, the polypropylene composition B and the polypropylene composition B' each comprise 5-20 wt% of the thermal adhesion enhancer y, such as 5 wt%, 15 wt%, 20 wt%, and any two values or any interval between any two values.
[0025] More preferably, the polypropylene composition B and the polypropylene composition B' each comprise 10-50 wt% of the flame retardant n, for example 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt%, and any two values or any interval between any two values.
[0026] According to some preferred embodiments of the present invention, the homopolypropylene a has: a melting point of 150-170°C, preferably 160-170°C; and / or a melt flow rate at 230°C and a load of 2.16 kg of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, further preferably 2.5-18 g / 10 min; and / or an isotacticity (mm) of not less than 96%.
[0027] According to some preferred embodiments of the present invention, the impact-resistant copolymerized polypropylene b has: the melting point of the impact-resistant copolymerized polypropylene b is 150-170°C: and / or the monomer of the impact-resistant copolymerized polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or the melt flow rate of the impact-resistant copolymerized polypropylene b at 230°C and a load of 2.16 kg is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and further preferably 2.5-18 g / 10 min; and / or the cantilever beam impact strength of the impact-resistant copolymerized polypropylene b is not less than 20 KJ / m 2 (Test conditions: 23℃).
[0028] According to the research conducted by the inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the sheet preparation process, so the sheet also has good tensile properties.
[0029] According to some preferred embodiments of the present invention, the random copolymer polypropylene x has: a melting point of 110-150°C, preferably 120-140°C; and / or a melt flow rate at 230°C and a load of 2.16 kg of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, further preferably 3-18 g / 10 min; and / or a molecular weight distribution Mw / Mn of 5-12, preferably 7-10; and / or a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
[0030] According to some preferred embodiments of the present invention, the thermal adhesion enhancer y has: a melting point or a viscosity flow temperature of 70-110°C; and / or a melt flow rate at 190°C and a load of 2.16kg of 0.5-50g / 10min, preferably 1-20g / 10min, and further preferably 1-18g / 10min; and / or, selected from one or more of polyolefin elastomers, EPDM rubber, SEBS, SBS, EVA, and petroleum resins; preferably, a polyolefin elastomer and / or a petroleum resin; more preferably, the polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably an α-olefin of C4-C12, more preferably 1-butene and / or 1-octene; and / or, the petroleum resin is a hydrogenated petroleum resin of C5 and / or C9 with a softening point of 100-150°C; preferably a cyclopentadiene type resin.
[0031] According to the research conducted by the present inventors, when the melt mass flow rate and polymer composition ratio of the polypropylene compositions B and B' are within the preferred range, the low melting point random copolymer polypropylene x and thermal bonding enhancer y in the composition can significantly reduce the hot pressing temperature and broaden the hot pressing temperature window, and the thermal bonding enhancer y provides the sheet with good bonding properties, which can further improve the interlayer peeling strength.
[0032] According to some preferred embodiments of the present invention, the layer A further contains a β-crystal nucleating agent; preferably,
[0033] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.
[0034] According to some preferred embodiments of the present invention, relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by weight, and any two values or any interval between any two values.
[0035] According to some preferred embodiments of the present invention, the flame retardant m and the flame retardant n are the same or different, and each is selected from one or more of the following: organic or inorganic compounds containing flame retardant elements and their polymers, inorganic substances and / or metal hydroxides that are stable at high temperatures; preferably, the flame retardant is selected from at least one of halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants, boron flame retardants, antimony flame retardants, biomass flame retardants, intumescent flame retardants, hydroxides and hydrates of oxides.
[0036] In order to better explain the present invention, the flame retardant m and the flame retardant n are described as follows: the types of the flame retardant m and the flame retardant n are not particularly limited, and can be a single component or a composite of multiple components, for example, organic or inorganic compounds and polymers containing flame retardant elements such as halogen, phosphorus, nitrogen, boron, antimony, etc., generally, the weight fraction of the flame retardant element in the flame retardant is 1-99wt%, preferably 5-90wt%; and inorganic substances and metal hydroxides that are stable at high temperatures. Preferably, the flame retardant is selected from at least one of halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants, boron flame retardants, antimony flame retardants, biomass flame retardants, intumescent flame retardants, hydroxides, and hydrates of oxides. Further, the halogen flame retardant includes at least one of decabromodiphenylethane, brominated epoxy resin, brominated polystyrene, substituted triazine, decabromodiphenyl ether, tetrabromobisphenol A, tetrabromophthalic anhydride, octabromoether, octabromodiphenyl ether, brominated epoxy resin, and brominated styrene-butadiene-styrene copolymer SBS; the phosphorus flame retardant can be red phosphorus, phosphoric acid, phosphate, hypophosphorous acid, hypophosphite, ammonium phosphate, phosphite, pyrophosphate, polyphosphate, phosphate ester, phosphite, organic phosphorus salt, ammonium polyphosphate, and phosphorus heterocyclic compounds and polymer phosphorus (phosphonic) esters, preferably aluminum hypophosphite and its alkylated The invention relates to a flame retardant comprising at least one of a modified substance, a pyrophosphate, and an ammonium polyphosphate; the nitrogen flame retardant includes melamine and its derivatives and related heterocyclic compounds, piperazine and its modified substances, preferably at least one of melamine and its modified substances, melamine salts, dicyandiamide, piperazine and its modified substances; the boron flame retardant may be boric acid and borates, preferably at least one of boric acid, ammonium borate and zinc borate; the antimony flame retardant may be at least one of antimony trioxide, antimony pentoxide and sodium antimonate; the hydrate of the hydroxide and the oxide may be at least one of the hydroxide of aluminum, magnesium, boron, zinc and the layered double metal hydroxide. The flame retardant composed of multiple components may also include at least one of pentaerythritol and its dimer, trimer, butanethritol, cyclohexanehexol, sorbitol, glucose, maltose and starch. Preferably, the composite flame retardant also includes an anti-dripping agent.
[0037] According to some preferred embodiments of the present invention, the BAB' layer structure of the flame retardant polypropylene sheet is obtained by coextruding layer A raw material comprising polypropylene composition A, layer B raw material comprising polypropylene composition B, and layer B' raw material comprising polypropylene composition B'.
[0038] According to the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'. In a preferred embodiment of the present invention, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene compositions B and B'; preferably, the melting point of the homopolymerized polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymerized polypropylene x in the polypropylene compositions B and B', and preferably the temperature difference of the corresponding melting points is greater than or equal to 10°C; and / or, the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B, and the difference between the melting point of the polypropylene composition A and the melting point of the polypropylene composition B' are each greater than or equal to 5°C, preferably greater than or equal to 10°C, and more preferably greater than or equal to 20°C. In such preferred embodiments, the inventors of the present invention surprisingly found that the obtained polypropylene sheet is subjected to hot pressing to obtain a polypropylene composite material, and the polypropylene composite material has more excellent mechanical properties and better interlayer peeling strength, even at a lower hot pressing temperature and a wider hot pressing temperature range, the obtained polypropylene composite material has a higher interlayer peeling strength.
[0039] According to the research of the present inventors, when the melt mass flow rate, polymer composition ratio and thickness distribution of the film layers B, B' of the polypropylene composition A and the polypropylene combinations B, B' are within the preferred range, the sheet preparation process can be made smoother, thereby making the sheet have better uniformity, tensile strength, impact performance and interlayer peeling strength.
[0040] In a second aspect, the object of the present invention is to provide a method for preparing the flame-retardant polypropylene sheet described in the first aspect, comprising co-extruding, casting or calendering, and stretching a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B' according to a BAB' structure to obtain the flame-retardant polypropylene sheet.
[0041] According to some preferred embodiments of the present invention, the preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the optional flame retardant m. The conditions and equipment for melt blending the polypropylene composition A are the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 150-170°C, and the equipment is preferably a twin-screw extruder.
[0042] According to some preferred embodiments of the present invention, the preparation of the raw materials of layer B and layer B' comprises melt blending the components including the random copolymer polypropylene x, the thermal adhesion enhancer y and the optional flame retardant n. The conditions and equipment for melt blending the polypropylene compositions B and B' are the conditions and equipment for melt blending of polyolefins in the prior art, preferably, the melting temperature is 110-150°C, and the equipment is preferably a twin-screw extruder.
[0043] Preferably, the co-extrusion and casting temperatures are independently selected from 200-240°C.
[0044] Preferably, the calendering temperature is 50-70°C.
[0045] The selection range of stretching conditions is relatively wide. In a preferred embodiment of the present invention, the stretching conditions include: the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is 90-165°C, preferably 90-140°C, and further preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0046] According to some embodiments of the present invention, polypropylene composition A, polypropylene composition B, B' are co-extruded according to the BAB' structure and cast or calendered to obtain a polypropylene co-extruded sheet. The process of the extrusion calendering method may include passing the polypropylene co-extruded sheet through a calendering roller and a traction roller in sequence, and then solid phase stretching, trimming and winding to obtain the sheet. The temperature of the extrusion casting is 200-230°C, and the temperature of the calendering roller is 50-70°C. The specific process of preparing the film by the extrusion calendering method is a commonly used choice in the art and will not be repeated here.
[0047] In a third aspect, the present invention aims to provide a flame retardant polypropylene fabric, which is a three-dimensional polypropylene fabric obtained by weaving the flame retardant polypropylene sheet described in the first aspect;
[0048] Preferably, the flame retardant polypropylene fabric is obtained by slitting and weaving the flame retardant polypropylene sheet; and / or the flame retardant polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
[0049] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then woven to obtain the polypropylene fabric.
[0050] In a fourth aspect, the present invention aims to provide a flame retardant polypropylene composite material, wherein the flame retardant polypropylene composite material is prepared by hot pressing multiple layers of the flame retardant polypropylene sheets described in the first aspect and / or the flame retardant polypropylene fabric described in the second aspect.
[0051] Preferably, the flame retardant polypropylene composite material is prepared by thermally pressing multiple layers of the flame retardant polypropylene sheets or the flame retardant polypropylene fabric.
[0052] Preferably, the multi-layer flame retardant polypropylene sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions.
[0053] Preferably, the multiple layers of flame retardant polypropylene fabric are stacked from top to bottom with the warp direction being 0-90° with the warp direction being the other direction.
[0054] Preferably, the number of layers of the multi-layer flame retardant polypropylene sheet and / or the multi-layer flame retardant polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers; most preferably 4-100 layers.
[0055] According to some preferred embodiments of the present invention, the flame retardant polypropylene composite material comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the flame-retardant polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;
[0056] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i ,
[0057] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.
[0058] According to the present invention, in the structure of the polypropylene composite material, the upper i-th group and the lower i-th group may be the same or different.
[0059] According to some preferred embodiments of the present invention, the polypropylene composition Ai Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is 5°C or more, preferably 10°C or more, and more preferably 20°C or more.
[0060] According to the present invention, the core layers in each polypropylene sheet unit can be made of the same material or different materials. There is no particular limitation on this. As long as A i The melting point is greater than that of the polypropylene composition B i , polypropylene composition B' i The melting point can achieve better technical effects.
[0061] According to some preferred embodiments of the present invention, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.
[0062] According to the present invention, the total number of stacked groups of the polypropylene sheet unit group is 2n-1. The present invention has a wide selection range for the total number of stacked groups of the polypropylene sheet unit group. In a preferred embodiment of the present invention, 2≤n≤100 is selected, more preferably, 2≤n≤50, and further preferably, 2≤n≤30.
[0063] According to the present invention, the selection range of the number of polypropylene sheet units included in each polypropylene sheet unit group is relatively wide. In a preferred embodiment of the present invention, each polypropylene sheet unit group independently includes 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.
[0064] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.
[0065] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the polypropylene composite material can be B from bottom to top. n A n B' n ……B i A i B' i ...B2A2B'2, B1A1B'1, B2A2B'2...B i Ai B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.
[0066] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the polypropylene composite material can be sequentially as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B'2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.
[0067] In a preferred embodiment of the present invention, the flame retardant polypropylene composite material has at least one of the following characteristics:
[0068] Longitudinal tensile strength ≥110MPa, preferably ≥130MPa;
[0069] Interlayer peel strength ≥1N / mm, preferably ≥1.2N / mm;
[0070] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the interlayer peel strength is measured according to the method specified in GB / T2358-98. The corresponding specimens in the above two tests are the standard specimens required in the above-mentioned test standards.
[0071] When the polypropylene composite material is obtained by hot pressing 24 layers of polypropylene fabrics and has a thickness of about 1.6 mm, the drop weight impact strength is ≥200 J, preferably ≥220 J.
[0072] The drop weight impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.
[0073] In a fifth aspect, the present invention aims to provide a method for preparing the flame-retardant polypropylene composite material according to the fourth aspect, the method comprising laminating and hot-pressing the flame-retardant polypropylene sheet and / or the flame-retardant polypropylene fabric, and then cooling and shaping to form the flame-retardant polypropylene composite material. Preferably,
[0074] Preferably, the conditions of the preparation method of the flame retardant polypropylene composite material include: the temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, the pressure of the hot pressing fusion is 2-10MPa; and / or, the preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, the cooling and setting pressure is 2-8MPa, and the cooling and setting time is 30-700s; and / or, the number of layers of the flame retardant polypropylene sheet and / or the flame retardant polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers; and / or, adjacent layers of the flame retardant polypropylene fabric laminate are placed at 0-90° between the warp and the warp; and / or, adjacent layers of the flame retardant polypropylene sheet laminate are placed at 0-90° along their respective machine directions.
[0075] As an example, in some preferred embodiments of the present invention, the method for preparing the high-strength and high-impact polypropylene composite material comprises the following steps:
[0076] Step a: co-extrude the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure and cast or calender to obtain a polypropylene co-extruded sheet; preferably, the extrusion casting or calendering temperature is 200-240° C., and the temperature of the calendering roller is 50-70° C.;
[0077] Step b: stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; the stretching method is free stretching, and / or solid phase stretching, and / or multi-stage stretching; the stretching temperature is preferably 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times, preferably 2-15 times.
[0078] Step c: cutting the polypropylene stretched sheet to prepare polypropylene flat strips, and weaving the flat strips to prepare polypropylene fabrics; preferably, the width of the polypropylene flat strips is 2-5 mm, and the polypropylene fabrics include plain weave, twill, satin weave or other three-dimensional polypropylene fabrics;
[0079] Step d: stacking the polypropylene fabrics in sequence, hot pressing and fusing them, and then cooling and shaping them to form a polypropylene composite material; preferably, in the step d, the hot pressing conditions are: hot pressing temperature 115-170°C, preferably 115-159°C, and more preferably 140-159°C; hot pressing pressure 2-10MPa, preheating time 5-600s, hot pressing time 1-600s, preferably 10-500s, cooling pressure 2-8MPa, cooling time 30-700s; preferably, adjacent polypropylene fabrics in the polypropylene composite material can be placed at 0-90° between the warp direction and the warp direction.
[0080] According to some embodiments of the present invention, in step c, a high-speed slitting machine with multiple blades can be used for cutting to obtain an oriented polypropylene flat ribbon with a width of 2-5 mm; a commercial weaving machine is used to weave the oriented flat ribbon according to the designed fabric structure to obtain plain, twill, satin or other three-dimensional polypropylene fabrics.
[0081] According to the present invention, in a preferred specific embodiment, the pressure is preferably maintained continuously during the hot pressing and cooling process without being reduced. The hot pressing process is carried out continuously, and preferably a continuous hot pressing composite material molding equipment consisting of a preheating machine, a crawler-type continuous flat hot press, a crawler-type continuous flat cooling press, a sheet cutting machine and a sheet stacking machine arranged in sequence is used; preferably, the crawler-type continuous flat hot press has a preheating unit, an independent heating and pressurizing unit, an air cooling unit and a lifting mechanism.
[0082] During the preparation, the polypropylene sheet and / or the polypropylene fabric are stacked in sequence and then preheated by a preheater. The preheated samples are sequentially hot-pressed and fused by a crawler-type flat hot press, and then cooled and shaped by a crawler-type continuous flat cooling press to form a polypropylene composite material, i.e., a stacked hot-pressed product. Afterwards, the sheets are sliced by a sheet cutter as needed, and the hot-pressed products are stacked and arranged by a sheet stacker. The hot-pressing temperature is controlled by a preheating unit, an independent heating and pressurizing unit, and an air-cooling unit in the crawler-type flat hot press, and the hot-pressing pressure is controlled by a lifting mechanism. According to the research of the inventors, when the preparation process parameters are within a preferred range, preferably when the preparation equipment is used to prepare the polymer composite material, the polymer composite material has better tensile strength, impact resistance, and interlayer peeling strength.
[0083] In a sixth aspect, the purpose of the present invention is to provide an application of the flame-retardant polypropylene sheet described in the first aspect, the flame-retardant polypropylene fabric described in the third aspect, the flame-retardant polypropylene composite material described in the fourth aspect, and the flame-retardant polypropylene composite material prepared by the preparation method described in the fifth aspect in the fields of electrical component packaging, automobile manufacturing, military materials and consumer goods.
[0084] According to a specific embodiment of the present invention, the material fields include electrical and electronics industry, luggage and transportation industry, shoemaking industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.
[0085] Compared with the prior art, the present invention has the following beneficial effects:
[0086] (1) The flame-retardant polypropylene composite material of the present invention has good tensile strength, impact resistance and interlayer peeling strength;
[0087] The flame retardant polypropylene composite material has the following characteristics:
[0088] The longitudinal (MD) tensile strength is ≥110MPa, preferably ≥130MPa; the interlayer peel strength is ≥1N / mm, preferably ≥1.2N / mm; the oxygen index is ≥26%, preferably ≥28%; the UL94 vertical combustion reaches V-1 level, preferably reaches V-0 level; when the composite material is only composed of 24 layers of polypropylene fabrics hot-pressed and the thickness is about 1.6mm, the drop hammer impact strength is ≥200J, preferably ≥220J.
[0089] (2) The flame-retardant polypropylene composite material of the present invention can be prepared at a relatively low hot pressing temperature and within a relatively wide hot pressing temperature range, which effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high-temperature operation. At the same time, when prepared at a relatively low hot pressing temperature, it still has good interlayer peeling strength.
[0090] (3) The preparation method can reduce the hot pressing operation time, while improving production efficiency and reducing production energy consumption.
[0091] (4) The present invention reduces the hot pressing temperature and expands the hot pressing temperature range to 50°C; it effectively reduces the energy consumption of the equipment and the damage to the composite material caused by high temperature operation.
[0092] (5) The flame-retardant polypropylene sheet, flame-retardant polypropylene fabric, and high-strength and high-impact flame-retardant polypropylene composite material of the present invention are suitable for application in thin plates, films, and fabrics while maintaining the mechanical properties of the flame-retardant polypropylene composite material, thereby broadening the application scenarios of flame-retardant polypropylene. DETAILED DESCRIPTION
[0093] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0094] In the following examples and comparative examples:
[0095] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model was HRPC-800 three-layer co-extrusion plastic stretching sheet production line.
[0096] The properties of the polypropylene composition and sheet were tested according to the following methods, and the film test results are shown in Table 1:
[0097] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682-2000, where the test temperature is 230°C and the load is 2.16 kg;
[0098] (2) Melting point: measured according to the method specified in GB / T 28724-2012;
[0099] (3) Tensile strength: measured according to the method specified in GB / T1040.1-2018;
[0100] (4) Drop weight impact strength: measured according to the method specified in GB / T14153-1993;
[0101] (5) Interlayer peel strength: measured according to the method specified in QB / T2358-98;
[0102] (6) Vertical combustion: measured according to the method specified in GN / T 2408-2008;
[0103] (7) Limiting oxygen index: measured according to the method specified in GB / T 2406.1-2008.
[0104] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.
[0105] Example 1
[0106] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0107] (1) Preparation of polypropylene composition A:
[0108] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry (under 23°C test conditions, the impact strength is 23kJ / m 2 ), ethylene content of 11%wt, melt flow rate of 2.0g / 10min, melting point of 155°C; flame retardant m is a composition of ammonium polyphosphate and pentaerythritol, purchased from Jinan Haobang Chemical Co., Ltd. The weight ratio of ammonium polyphosphate to pentaerythritol in component m is 2:1.
[0109] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 64 parts by weight, the mass fraction Wb of component b is 16 parts by weight, and the mass fraction Wm of component m is 20 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B and 0.3 parts by weight of blendex 6530 anti-dripping agent are added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melted and mixed evenly, extruded, granulated and dried, a polypropylene composition pellet A is obtained. The melting point of the polypropylene composition A is 158°C after testing.
[0110] (2) Preparation of polypropylene composition B:
[0111] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C and a melt flow rate of 6.6 g / 10 min; component y is a polyolefin elastomer with a grade of 6102, purchased from Exxon, which is an ethylene-propylene copolymer with an ethylene content of 16%wt and a melt flow rate of 1.4 g / 10 min at 230°C and a load of 2.16 kg; flame retardant n is a composition of ammonium polyphosphate and pentaerythritol. The weight ratio of ammonium polyphosphate to pentaerythritol in component n is 2:1.
[0112] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wn of component n is 30 parts by weight. The other steps are the same as step (1), and finally a polypropylene composition B pellet is obtained, and its melting point is 138° C. after detection;
[0113] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0114] The pellets of polypropylene composition A and polypropylene composition B obtained in the above steps (1) and (2) are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering machine, and the polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion casting machine.
[0115] After the pellets are co-extruded and compounded out from the die of the extruder, they are sequentially passed through a calendering roller and a traction roller, and then subjected to solid phase stretching, edge cutting and winding, thereby obtaining the sheet.
[0116] The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 55°C. The temperature during the solid phase stretching was 135°C, the stretching rate was 2m / min, and the stretching ratio was 6 times. After stretching, the film was rolled up to form a polypropylene sheet (composite film), which consisted of an upper surface layer (film layer A), a core layer (film layer A), and a lower surface layer (film layer B).
[0117] The thickness of the polypropylene sheet (composite film) is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.
[0118] (4) Preparation of polypropylene fabric:
[0119] The three-layer co-extruded polypropylene sheet obtained in the above step (3) is cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon is woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave polypropylene fabric.
[0120] (5) Preparation of polypropylene composite materials:
[0121] The polypropylene fabrics obtained in the above step (4) are laminated and hot pressed in sequence to form a laminated polypropylene sheet. The laminated polypropylene sheet includes 24 layers of polypropylene fabrics, and the polypropylene fabrics are placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 180s, hot pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.67mm.
[0122] Example 2
[0123] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0124] (1) Preparation of polypropylene composition A:
[0125] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an impact strength of 25kJ / m under 23°C test conditions. 2 , ethylene content is 8%wt, melt flow rate is 3.2g / 10min, melting point is 155°C. Flame retardant m is a composition of ammonium polyphosphate and pentaerythritol. The weight ratio of ammonium polyphosphate to pentaerythritol in component m is 2:1.
[0126] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 56 parts by weight, the mass fraction Wb of component b is 24 parts by weight, and the mass fraction Wm of component m is 20 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade of VP101B and 0.3 parts by weight of blendex 6530 anti-dripping agent are added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P Company. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melted and mixed evenly, extruded, granulated and dried, a polypropylene composition pellet A is obtained. The melting point of the polypropylene composition A is 162°C after testing.
[0127] (2) Preparation of polypropylene composition B:
[0128] Component x is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 134°C, an ethylene-propylene-butene terpolymer, and a melt flow rate of 5.2 g / 10 min; component y is a polyolefin elastomer produced by Sinopec Beijing Research Institute of Chemical Industry, an ethylene-propylene copolymer, with an ethylene content of 15% wt, a melting point of 105°C, and a melt flow rate of 9 g / 10 min at 230°C and a load of 2.16 kg; flame retardant n is a composition of ammonium polyphosphate and pentaerythritol. The weight ratio of ammonium polyphosphate to pentaerythritol in component n is 2:1.
[0129] The components prepared above are weighed and mixed according to the proportion, wherein the mass fraction Wx of component x is 60 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and the mass fraction Wn of component n is 30 parts by weight. The other steps are the same as step (1), and finally polypropylene composition B pellets are obtained. The melting point of the polypropylene composition B is 132°C after testing.
[0130] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0131] The preparation process is the same as step (3) of Example 1.
[0132] (4) Preparation of polypropylene fabric:
[0133] The preparation process is the same as step (4) of Example 1.
[0134] (5) Preparation of polypropylene composite materials:
[0135] The preparation process is the same as step (5) of Example 1.
[0136] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0137] Example 3
[0138] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0139] (1) Preparation of polypropylene composition A:
[0140] The same as Example 1, except that the flame retardant m is a composition of decabromodiphenylethane and antimony trioxide, purchased from Jinan Taixing Fine Chemical Co., Ltd. The weight ratio of decabromodiphenylethane to antimony trioxide in component m is 5:1. 0.05 weight parts of β-crystal nucleating agent with the grade of VP101B and 0.3 weight parts of blendex 6530 anti-dripping agent are added. Polypropylene composition A pellets are obtained, and the melting point of polypropylene composition A is 159°C after testing.
[0141] (2) Preparation of polypropylene composition B:
[0142] The same as Example 1, except that the flame retardant n is a composition of decabromodiphenylethane and antimony trioxide, purchased from Jinan Taixing Fine Chemical Co., Ltd. The weight ratio of decabromodiphenylethane to antimony trioxide in component n is 5:1, and finally a polypropylene composition B pellet is obtained. The melting point of the polypropylene composition B is 140°C after testing.
[0143] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0144] The preparation process is the same as step (3) of Example 1.
[0145] (4) Preparation of polypropylene fabric:
[0146] The preparation process is the same as step (4) of Example 1.
[0147] (5) Preparation of polypropylene composite materials:
[0148] The preparation process is the same as step (5) of Example 1.
[0149] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0150] Example 4
[0151] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0152] (1) Preparation of polypropylene composition A:
[0153] The preparation process is the same as step (1) of Example 1.
[0154] (2) Preparation of polypropylene composition B:
[0155] The preparation process is the same as step (2) of Example 1. The difference is that in the preparation of polypropylene composition B, the mass fraction Wx of component x is 85 parts by weight, the mass fraction Wy of component y is 15 parts by weight, and no flame retardant n is added.
[0156] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0157] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.
[0158] (4) Preparation of polypropylene fabric:
[0159] The preparation process is the same as step (4) of Example 1.
[0160] (5) Preparation of polypropylene composite materials:
[0161] The preparation process is the same as step (5) of Example 1.
[0162] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0163] Example 5
[0164] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0165] (1) Preparation of polypropylene composition A:
[0166] The preparation process is the same as step (1) of Example 1.
[0167] (2) Preparation of polypropylene composition B:
[0168] The preparation process is the same as step (2) of Example 1.
[0169] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0170] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 70% of the total thickness of the sheet.
[0171] (4) Preparation of polypropylene fabric:
[0172] The preparation process is the same as step (4) of Example 1.
[0173] (5) Preparation of polypropylene composite materials:
[0174] The preparation process is the same as step (5) of Example 1.
[0175] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0176] Example 6
[0177] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0178] (1) Preparation of polypropylene composition A:
[0179] The preparation process is the same as step (1) of Example 1.
[0180] (2) Preparation of polypropylene composition B:
[0181] The preparation process is the same as step (2) of Example 1.
[0182] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0183] The preparation process is the same as step (3) of Example 1.
[0184] (4) Preparation of polypropylene fabric:
[0185] The preparation process is the same as step (4) of Example 1.
[0186] (5) Preparation of polypropylene composite materials:
[0187] The main steps are the same as those in Example 1. The laminated polypropylene sheet includes two layers of polypropylene fabric. The hot pressing conditions are: temperature 140°C, hot pressing pressure 2MPa, preheating time 120s, hot pressing time 10s, cooling time 300s. The thickness of the prepared polypropylene composite material is 129μm.
[0188] Example 7
[0189] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0190] (1) Preparation of polypropylene composition A:
[0191] The preparation process is the same as step (1) of Example 1.
[0192] (2) Preparation of polypropylene composition B:
[0193] The preparation process is the same as step (2) of Example 1.
[0194] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0195] The preparation process is the same as step (3) of Example 1.
[0196] (4) Preparation of polypropylene fabric:
[0197] The preparation process is the same as step (4) of Example 1.
[0198] (5) Preparation of polypropylene composite materials:
[0199] The main steps are the same as those in Example 1. The laminated polypropylene sheet includes 100 layers of polypropylene fabric. The hot pressing conditions used are: 159°C, hot pressing pressure of 10 MPa, preheating time of 300 s, hot pressing time of 300 s, and cooling time of 700 s. The thickness of the prepared polypropylene composite material is 7.23 mm.
[0200] Example 8
[0201] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0202] (1) Polypropylene composition A i Preparation:
[0203] The preparation process is the same as step (1) of Example 1.
[0204] (2) Polypropylene composition B i Preparation:
[0205] The main preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:
[0206] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min and a melting point of 140°C; component y is a polyolefin elastomer with a brand number of 6102, purchased from Exxon, and is an ethylene-propylene copolymer.
[0207] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y+n=B i, i=1, 2, 3), after testing, the melting point of B1 is 128°C, the melting point of B2 is 134°C, and the melting point of B3 is 138°C.
[0208] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0209] The preparation process is the same as step (3) of Example 1. Sheets B1AB1, B2AB2, and B3AB3 are obtained respectively.
[0210] (4) Preparation of polypropylene fabric:
[0211] The preparation process is the same as step (4) of Example 1. Plain woven polypropylene fabrics B1AB1, B2AB2, and B3AB3 are obtained.
[0212] (5) Preparation of polypropylene composite materials:
[0213] The polypropylene fabrics obtained in the above step (4) are stacked in order, from bottom to top, B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, and the total number of stacked layers is 5. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 90s, hot pressing time 90s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 410μm.
[0214] Example 9
[0215] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, and polypropylene composite material provided by the present invention.
[0216] (1) Polypropylene composition A i Preparation:
[0217] The preparation process is the same as step (1) of Example 1.
[0218] (2) Polypropylene composition B i Preparation:
[0219] The main preparation process is the same as step (2) of Example 1. The difference is that component B i and x i The materials are as follows:
[0220] Components x1-x4 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 128°C; components x5-x8 are random copolymer polypropylenes produced by Sinopec Beijing Research Institute of Chemical Industry, which are ethylene-propylene-butene terpolymers with a melting point of 135°C; components x9-x 12 It is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a melting point of 142°C; among them, components x1-x 12 The molecular weight distribution Mw / Mn is between 7 and 10, and the components x1-x 12 The melt flow rate is 1-20g / 10min.
[0221] Finally, the polypropylene composition B is obtained. i Granules (i.e. x i +y+n=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12). After testing, the melting points of B1-B4 are 126°C, the melting points of B5-B8 are 133°C, and the melting points of B9-B 12 The melting point is 140°C.
[0222] (3) Preparation of three-layer co-extruded polypropylene sheet:
[0223] The preparation process is the same as step (3) of Example 1.
[0224] (4) Preparation of polypropylene fabric:
[0225] The preparation process is the same as step (4) of Example 1.
[0226] (5) Preparation of polypropylene composite materials:
[0227] The polypropylene fabrics obtained in step (4) are stacked in order, from bottom to top: B 12 AB 12… B3AB3, B2AB2, B1AB1, B2AB2, B3AB3,…B 12 AB 12 The total number of stacked layers is 23, and the laminated polypropylene fabric is hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed in a direction of 90 degrees between the warp and the warp. The hot pressing conditions used are: temperature 150°C, hot pressing pressure 5MPa, preheating time 160s, hot pressing time 160s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.57mm.
[0228] Comparative Example 1
[0229] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0230] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0231] Comparative Example 2
[0232] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition B was used for extrusion casting into a single-layer film with a thickness of 80 μm. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0233] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0234] Comparative Example 3
[0235] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 3, except that the polypropylene composition A contained only component b and component m, the mass fraction Wb of component b was 75 parts by weight, and the mass fraction Wm of component m was 25 parts by weight. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0236] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0237] Comparative Example 4
[0238] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 3, except that the polypropylene composition B contained only component y and component n, the mass fraction Wy of component y was 75 parts by weight, and the mass fraction Wn of component n was 25 parts by weight. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0239] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0240] Comparative Example 5
[0241] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A did not contain component m, and the polypropylene composition B did not contain component n. A polypropylene fabric and a polypropylene composite material were prepared according to the method of Example 1.
[0242] The thickness of the prepared polypropylene composite material is close to that of Example 1.
[0243] Comparative Example 6
[0244] According to the method of Example 8, a three-layer coextruded polypropylene sheet and a polypropylene fabric were prepared.
[0245] The difference lies in the preparation of the polypropylene composite material. The prepared polypropylene fabrics are stacked in sequence, and the stacking order is: from bottom to top, B1A1B1, B2A2B2, B3A3B3, B2A2B2, B1A1B1 (i.e., the melting point of B1 is 128°C, the melting point of B2 is 134°C, and the melting point of B3 is 138°C). The total number of stacked layers is 5 layers. The stacked polypropylene fabrics are hot-pressed and fused, and then cooled and shaped to form a polypropylene composite material. The polypropylene fabric is placed at 90° between the warp and the warp. The hot pressing conditions used are: temperature 145°C, hot pressing pressure 5MPa, preheating time 110s, hot pressing time 110s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 418μm.
[0246] Experimental example
[0247] The polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following method. The test results are shown in Table 1.
[0248] (1) Tensile strength: Sample preparation and determination shall be carried out in accordance with the method specified in GB / T1040.1-2018.
[0249] (2) Interlayer peel strength: Sample preparation and measurement shall be carried out according to the method specified in QB / T2358-98.
[0250] (3) Drop hammer impact strength: measured according to the method specified in GB / T14153-1993. The thicknesses of the polypropylene composite materials obtained in Examples 1-5, Example 9, and Comparative Examples 1-5 are close to each other, about 1.6 mm, and are all within the range of 1.6 mm ± 1 mm.
[0251] (4) Vertical combustion: The test was conducted according to the method specified in GN / T 2408-2008. The thickness of the polypropylene composite materials obtained in Examples 1-5, Example 9, and Comparative Examples 1-5 were similar, about 1.6 mm; 12 samples of Example 6 were stacked and hot pressed to obtain samples with a thickness of about 1.6 mm; 4 samples of Example 8 and Comparative Example 6 were stacked and hot pressed to obtain samples with a thickness of about 1.6 mm; the sample of Example 7 was cut into 1.6 mm samples.
[0252] (5) Limiting oxygen index: measured according to the method specified in GB / T 2406.1-2008.
[0253] Table 1
[0254]
[0255]
[0256] From the results of the examples in Table 1, it can be concluded that the flame-retardant polypropylene composite material prepared according to the present invention has good tensile properties, impact resistance and flame retardant properties, and has good interlayer peeling strength at a relatively low hot pressing temperature. The longitudinal (MD) tensile strength of the polypropylene composite sheet of the present invention is ≥110MPa, and the interlayer peeling strength is ≥1N / mm; when the polypropylene composite material is hot-pressed by 24 layers of polypropylene fabric, and the thickness is about 1.6mm, the drop hammer impact strength is ≥200J, reaching V-1 level, and preferably reaching V-0 level.
[0257] It can be seen from preferred embodiments 1-3 that the longitudinal (MD) tensile strength of the polypropylene composite material prepared by the present invention is ≥130 MPa, and the interlayer peel strength is ≥1.2 N / mm; when the polypropylene composite material is composed of 24 layers of polypropylene fabrics hot-pressed and has a thickness of about 1.6 mm, the drop weight impact strength is ≥220 J, and UL-94 reaches V-1 level.
[0258] It can be seen from Comparative Examples 1-5 that only using a single-layer sheet structure or using an interlayer ratio outside the scope of the present invention will lead to a decrease in the performance of the laminated polypropylene sheet or fabric. Using conditions outside the scope of the present invention will greatly reduce the tensile strength, impact properties, interlayer peel strength or flame retardant properties of the obtained polypropylene composite material.
[0259] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0260] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A flame retardant polypropylene sheet, comprising a layer A and layers B and B' located on both sides of the layer A, with a structure of BAB'; Wherein layer B and layer B' are the same or different, and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x, a thermal bonding enhancer y and an optional flame retardant n; layer A contains a polypropylene composition A, wherein the polypropylene composition A includes a homopolymer polypropylene a, an impact copolymer polypropylene b and an optional flame retardant m; in, The melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B', and the contents of the corresponding flame retardant m and flame retardant n in the polypropylene composition A, the polypropylene composition B and the polypropylene composition B' are not 0 at the same time.
2. The flame retardant polypropylene sheet according to claim 1, characterized in that: The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene composition B and the polypropylene composition B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10°C; and / or, Based on the total thickness of the flame retardant polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%; and / or, The difference between the melting points of the polypropylene composition A and the polypropylene composition B and the difference between the melting points of the polypropylene composition A and the polypropylene composition B' are each equal to or greater than 5°C, preferably equal to or greater than 10°C, more preferably equal to or greater than 20°C.
3. The flame retardant polypropylene sheet according to claim 1, characterized in that: Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 30-98wt% of homopolypropylene a, 1-50wt% of impact copolymer polypropylene b, and 0-60wt% of flame retardant m; preferably, the polypropylene composition A comprises 40-80wt% of homopolypropylene a, 5-30wt% of impact copolymer polypropylene b, and 2-50wt% of flame retardant m; and / or, Based on the total weight of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each include 30-98wt% of random copolymer polypropylene x, 1-50wt% of thermal adhesion enhancer y, and 0-60wt% of flame retardant n; preferably, the polypropylene composition B and the polypropylene composition B' each include 40-80wt% of random copolymer polypropylene x, 5-30wt% of thermal adhesion enhancer y, and 2-50wt% of flame retardant n.
4. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.
5. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .
6. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.
7. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The thermal bonding enhancer y has: The melting point or viscosity flow temperature is 70-110°C; and / or, The melt flow rate at 190°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 1-18 g / 10 min; and / or, One or more selected from polyolefin elastomer, EPDM rubber, SEBS, SBS, EVA, petroleum resin; preferably, polyolefin elastomer and / or petroleum resin; more preferably, The polyolefin elastomer is a copolymer elastomer of ethylene and propylene and / or α-olefin, the α-olefin is preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150°C; preferably a cyclopentadiene type resin.
8. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The BAB' sheet structure of the flame-retardant polypropylene sheet is obtained by co-extruding a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B'; and / or, The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.
9. The flame retardant polypropylene sheet according to any one of claims 1 to 3, characterized in that: The flame retardant m and the flame retardant n are the same or different, and each is selected from one or more of the following: organic or inorganic compounds containing flame retardant elements and polymers thereof, inorganic substances and / or metal hydroxides that are stable at high temperatures; preferably, The flame retardant is selected from at least one of halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants, boron flame retardants, antimony flame retardants, biomass flame retardants, intumescent flame retardants, hydroxides and hydrates of oxides.
10. A method for preparing the flame-retardant polypropylene sheet according to any one of claims 1 to 9, comprising co-extruding, casting or calendering, and stretching a layer A raw material comprising a polypropylene composition A, a layer B raw material comprising a polypropylene composition B, and a layer B' raw material comprising a polypropylene composition B' according to a BAB' structure to obtain the flame-retardant polypropylene sheet.
11. The method for preparing the flame retardant polypropylene sheet according to claim 10, characterized in that: The preparation of the raw material of layer A comprises melt blending the components including the homopolypropylene a, the impact copolymer polypropylene b and the optional flame retardant m; and / or, The preparation of the raw materials of the layer B and the layer B' comprises melt blending the components including the random copolymer polypropylene x, the thermal adhesion enhancer y and the optional flame retardant n; and / or, The co-extrusion and casting temperatures are independently selected from 200-240° C.; and / or, The calendering temperature is 50-70°C; and / or, The stretching conditions include: the stretching temperature is 90-165° C., preferably 90-140° C., and more preferably 90-119° C.; and the stretching ratio is 1-20 times.
12. A flame retardant polypropylene fabric, a three-dimensional polypropylene fabric obtained by weaving the flame retardant polypropylene sheet according to any one of claims 1 to 9; Preferably, the flame retardant polypropylene fabric is obtained by slitting and weaving the flame retardant polypropylene sheet; and / or the flame retardant polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.
13. A flame-retardant polypropylene composite material, which is prepared by hot pressing multiple layers of the flame-retardant polypropylene sheet according to any one of claims 1 to 9 and / or the flame-retardant polypropylene fabric according to claim 12; preferably, The flame retardant polypropylene composite material is prepared by thermally pressing multiple layers of the flame retardant polypropylene sheets or the flame retardant polypropylene fabric; and / or, The multi-layer flame retardant polypropylene sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions; and / or, The multi-layer flame retardant polypropylene fabric is stacked from top to bottom with the warp direction being 0-90°; and / or, The number of layers of the multi-layer flame retardant polypropylene sheet and / or the multi-layer flame retardant polypropylene fabric is greater than or equal to 2 layers, more preferably 2-200 layers, and most preferably 4-100 layers.
14. The flame retardant polypropylene composite material according to claim 13, characterized in that: The flame retardant polypropylene composite material comprises a plurality of polypropylene sheet unit groups stacked in sequence; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the flame-retardant polypropylene composite material is, from bottom to top, the nth group... the ith group... the second group, the first group, the second group... the ith group... the nth group, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than the average melting point of all outer layers in the i-1-th group.
15. The flame retardant polypropylene composite material according to claim 14, characterized in that: Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 2≤n≤100, preferably, 2≤n≤50; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.
16. A method for preparing a flame-retardant polypropylene composite material according to any one of claims 13 to 15, the method comprising laminating and hot-pressing the flame-retardant polypropylene sheet and / or the flame-retardant polypropylene fabric, and then cooling and shaping to form a flame-retardant polypropylene composite material; preferably, The temperature of the hot pressing fusion is 115-170°C, preferably 115-159°C, and more preferably 140-159°C; and / or, The pressure of the hot pressing fusion is 2-10 MPa; and / or, The preheating time of the hot pressing fusion is 5-600s, and the hot pressing time is 1-600s, preferably 10-500s; and / or, The cooling and shaping pressure is 2-8 MPa, and the cooling and shaping time is 30-700 s; and / or, The number of layers of the flame retardant polypropylene sheet and / or the flame retardant polypropylene fabric laminate is greater than or equal to 2 layers, preferably 2-200 layers; more preferably 4-100 layers; and / or, Adjacent layers of the flame retardant polypropylene fabric laminate are placed at an angle of 0-90° between the warp direction; and / or, Adjacent layers of the flame retardant polypropylene sheet laminate are placed at 0-90 degrees along their respective machine directions.
17. Application of the flame-retardant polypropylene sheet according to any one of claims 1 to 9, the flame-retardant polypropylene fabric according to claim 12, the flame-retardant polypropylene composite material according to any one of claims 13 to 15, and the flame-retardant polypropylene composite material prepared by the preparation method according to claim 16 in the fields of electrical component packaging, automobile manufacturing, military materials and consumer products.
Citation Information
Patent Citations
Polypropylene composite film as well as preparation method and application thereof
CN115991908A
Flame-retardant polypropylene composite film as well as preparation method and application thereof
CN115991910A
Propylene polymer-based composite film, preparation method therefor, and application thereof
WO2022083659A1