Tearable antistatic film and preparation method and application thereof
By introducing an antistatic thermocombination layer into the PE film, using materials such as linear polyethylene, low-density polyethylene, 1-butenyl polymer and EVA resin, a multi-layer structure tearable antistatic film is formed, which solves the problem of easy heat-combination after thermal bonding. The problem of tearing and adsorbing dust bacteria has achieved efficient anti-static and tearability, and is suitable for medical protection.
Patent Information
- Application Number
- CN202410958339.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing PE films are difficult to meet good tearability after thermal bonding, which are easy to tear and easily adsorb dust bacteria, bringing the risk of infection.
A tearable antistatic film with a multi-layer structure, including a conventional layer and an antistatic thermocoupling layer, is combined with materials such as linear polyethylene, low-density polyethylene, 1-butenyl polymer, EVA resin and antistatic masterbatch. It forms excellent antistatic, fracture strength and tearability after thermal bonding.
It achieves a film that is free of damage after thermal bonding and is easy to tear, has good antistatic properties, is suitable for medical sheeting and isolation clothing, reducing the risk of infection.
Smart Images

Figure CN118906606A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical polymer materials, and in particular to a tearable antistatic film and a preparation method and application thereof. Background Art
[0002] At present, in medical protection, with the enrichment of products, the functional requirements for products are also slowly increasing. Existing PE products are difficult to meet the requirements of good tearability after heat sealing. For example, the joints of PE films are easily torn when they are torn after heat sealing, which brings a lot of troubles to doctors during use. At the same time, some lint will be generated during tearing, which will also bring the risk of infection during use. At the same time, because PE has strong adsorption, it is easy to absorb some dust and bacteria, which will also bring some infection risks. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a tearable antistatic film and a preparation method and application thereof.
[0004] The technical solution adopted by the present invention to solve the technical problem is: to provide a tearable antistatic film, including a conventional layer, and an antistatic heat-sealing layer integrally composited on opposite sides of the conventional layer;
[0005] The conventional layer includes the following raw materials and their weight proportions: 40-75 parts of linear polyethylene, 24-57 parts of low-density polyethylene and 1-3 parts of anti-blocking masterbatch;
[0006] The antistatic heat-sealing layer includes raw materials and their mass proportions are as follows: 26-62 parts of linear polyethylene, 16-26 parts of low-density polyethylene, 10-20 parts of 1-butene-based polymer, 6-15 parts of EVA resin, 5-10 parts of antistatic masterbatch and 1-3 parts of anti-adhesion masterbatch.
[0007] In some embodiments, the density of the linear polyethylene is 0.91 g / cm 3 ~0.94g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.2g / 10min to 2.5g / 10min.
[0008] In some embodiments, the density of the low-density polyethylene is 0.91 g / cm 3 ~0.925g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.7 g / 10min to 2.3 g / 10min.
[0009] In some embodiments, the density of the 1-butene-based polymer is 0.91 g / cm 3 ~0.93g / cm 3The melt index is 3g / 10min~4g / 10min at a temperature of 190°C and a load of 2160g.
[0010] In some embodiments, the density of the EVA is 0.92 g / cm 3 ~0.95g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 2g / 10min to 3g / 10min.
[0011] In some embodiments, the density of the antistatic masterbatch is 0.93 g / cm 3 The melt index at a temperature of 190°C and a load of 2160 g is 6 g / 10 min.
[0012] In some embodiments, the density of the anti-blocking masterbatch is 1 g / cm 3 ~1.2g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 6g / 10min to 9g / 10min.
[0013] In some embodiments, the tearable antistatic film has a thickness of 30 μm to 200 μm; and the thickness ratio of the antistatic heat-sealing layer on one side of the conventional layer to the conventional layer is 0.8-1.5:1.
[0014] The present invention also provides a method for preparing a tearable antistatic film, comprising the following steps:
[0015] The raw materials of the conventional layer and the antistatic heat-sealing layer are heated, stirred and dried respectively, and then sent to the barrel of the film blowing machine, and co-extruded and blown by the extruder to form a composite tearable antistatic film, which is then cooled, shaped, pulled, slit and rolled.
[0016] The present invention also provides an application of a tearable antistatic film for medical drapes or isolation gowns.
[0017] The beneficial effects of the present invention are as follows: an antistatic heat-sealing layer is compounded on the outside of a conventional layer to form a multilayer film, which has excellent antistatic properties, breaking strength, and tearability after heat sealing, can meet the requirements of medical protection antistatic properties and tearability after heat sealing, and is simple and stable to prepare. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0019] Figure 1 Schematic diagram of the laminated structure of a tearable antistatic film according to an embodiment of the present invention. DETAILED DESCRIPTION
[0020] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.
[0021] like Figure 1 As shown, the tearable antistatic film according to an embodiment of the present invention includes a conventional layer 10 and an antistatic heat-sealing layer 20 integrally laminated on opposite sides of the conventional layer 10 .
[0022] The conventional layer 10 includes the following raw materials and their weight proportions: 40 to 75 parts of linear polyethylene, 24 to 57 parts of low-density polyethylene and 1 to 3 parts of anti-blocking masterbatch.
[0023] As a preferred embodiment, in the conventional layer 10, the density of the linear polyethylene is 0.91 g / cm 3 ~0.94g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.2g / 10min to 2.5g / 10min. The density of low-density polyethylene is 0.91g / cm 3 ~0.925g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.7 g / 10min to 2.3 g / 10min.
[0024] Furthermore, in the conventional layer 10, the degree of polymerization of the linear polyethylene may be 500-2000, and the degree of polymerization of the low-density polyethylene may be 1000-3000.
[0025] The density of anti-adhesion masterbatch is 1g / cm 3 ~1.2g / cm 3 , the melt index at a temperature of 190°C and a load of 2160g is 6g / 10min to 9g / 10min. Alternatively, the anti-adhesion masterbatch is made of a raw material compounded with at least one of diatomaceous earth, talc, kaolin and silicon dioxide and at least one of oleamide and erucic acid. For example, it is made of a raw material compounded with at least one of diatomaceous earth, talc, kaolin and silicon dioxide and oleamide; or, it is made of a raw material compounded with at least one of diatomaceous earth, talc, kaolin and silicon dioxide and erucic acid; or, it is made of a raw material compounded with at least one of diatomaceous earth, talc, kaolin and silicon dioxide and oleamide and erucic acid.
[0026] The antistatic heat-sealing layer 20 includes raw materials and their mass proportions as follows: 26-62 parts of linear polyethylene, 16-26 parts of low-density polyethylene, 10-20 parts of 1-butene-based polymer, 6-15 parts of EVA (ethylene-vinyl acetate copolymer) resin, 5-10 parts of antistatic masterbatch and 1-3 parts of anti-adhesion masterbatch.
[0027] The raw materials of the antistatic heat-sealing layer 20 are linear polyethylene, low-density polyethylene, 1-butene-based polymer and EVA resin, and an incompletely compatible blending system is used to control the heat-sealing tearability by mixing incompletely compatible dispersions into the continuous phase.
[0028] As a preferred embodiment, in the antistatic heat-sealing layer 20, the density of the linear polyethylene is 0.91 g / cm 3 ~0.94g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.2g / 10min to 2.5g / 10min. The density of low-density polyethylene is 0.91g / cm 3 ~0.925g / cm 3 The melt index at a temperature of 190°C and a load of 2160 g is 1.7 g / 10 min to 2.3 g / 10 min. The density of the 1-butene polymer is 0.91 g / cm 3 ~0.93g / cm 3 The melt index is 3g / 10min~4g / 10min at a temperature of 190°C and a load of 2160g. The density of EVA is 0.92g / cm 3 ~0.95g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 2g / 10min to 3g / 10min. The density of the antistatic masterbatch is 0.93g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 6g / 10min. The density of the anti-blocking masterbatch is 1g / cm 3 ~1.2g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 6g / 10min to 9g / 10min.
[0029] Furthermore, in the antistatic heat-sealing layer 20, the degree of polymerization of linear polyethylene may be 500-2000, the degree of polymerization of low-density polyethylene is 1000-3000, the degree of polymerization of 1-butene polymer is 300-5000, and the degree of polymerization of EVA (ethylene-vinyl acetate copolymer) is 200-1000.
[0030] The antistatic masterbatch is used as an antistatic agent to play an antistatic role. It can be selected from polyether antistatic agents or quaternary ammonium salt antistatic agents. The antistatic masterbatch can further be preferably made of polyether ester amide or a cationic quaternary ammonium salt antistatic agent with an amide structure.
[0031] The tearable antistatic film of the present invention can have a thickness of 30 μm to 200 μm. In the tearable antistatic film, the thickness ratio of the antistatic heat-sealing layer 20 on one side of the conventional layer 10 to the conventional layer 10 is 0.8 to 1.5:1; then, the total thickness ratio of the antistatic heat-sealing layer 20 on the opposite sides of the conventional layer 10 to the thickness of the conventional layer 10 is 1.6 to 3.0:1. It can be seen that the thickness of the antistatic heat-sealing layer 20 on one side can be greater than the thickness of the conventional layer 10, or less than the thickness of the conventional layer 10, or the same as the thickness of the conventional layer 10, that is, 1:1.
[0032] refer to Figure 1 In some embodiments, the method for preparing the tearable antistatic film of the present invention may include the following steps:
[0033] The raw materials of the conventional layer 10 and the antistatic heat-sealing layer 20 are heated, stirred and dried respectively, and then sent to the barrel of the film blowing machine, and co-extruded and blown by the extruder to form a composite tearable antistatic film, which is then cooled, shaped, pulled, slit and rolled.
[0034] Specifically, in the film blowing machine, the film blowing machine has three screw barrels. The raw materials of the conventional layer 10 are in the middle screw barrel, and the raw materials of the antistatic heat sealing layer 20 are in the screw barrels on both sides. After being plasticized and melted by the screw, under the pressure of the screw and the forward thrust of the screw, the molten raw materials in the screw barrel are transported to the die for inflation and cooling and forming. The outer layers on both sides are the antistatic heat sealing layer 20, and the middle is the conventional layer 10. The antistatic heat sealing layer 20 and the conventional layer 10 are an integrally formed film.
[0035] The working temperature of the screw is 105°C to 155°C, and the die head temperature of the casting machine is 130°C to 160°C.
[0036] The tearable antistatic film of the present invention is tearable and will not generate lint after being torn, and also has an antistatic function, and is suitable for medical drapes, isolation gowns, and the like.
[0037] The present invention will be further described below with reference to specific embodiments.
[0038] Example 1
[0039] Raw materials for the antistatic heat-sealing layer: 26 parts of linear polyethylene resin, 26 parts of low-density polyethylene, 20 parts of 1-butene-based polymer, 15 parts of EVA resin, 10 parts of antistatic masterbatch, and 3 parts of anti-blocking masterbatch. Raw materials for the conventional layer: 40 parts of linear polyethylene resin, 57 parts of low-density polyethylene, and 3 parts of anti-blocking masterbatch.
[0040] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0041] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0042] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 25.5N / 5cm, a MD breaking strength of 52.5N / 5cm, and a surface resistance of 1.2×10 10 Ω.
[0043] After the antistatic PE film is heat-sealed with the antistatic PE film, the heat-sealed part is not damaged after tearing and can be easily torn. After the antistatic PE film is heat-sealed with the conventional 100% PE (conventional polyethylene film), the heat-sealed part is not damaged after tearing and can be easily torn.
[0044] Example 2
[0045] Raw materials for the antistatic heat-sealing layer: 62 parts of linear polyethylene resin, 16 parts of low-density polyethylene, 10 parts of 1-butene-based polymer, 6 parts of EVA resin, 5 parts of antistatic masterbatch, and 1 part of anti-blocking masterbatch. Raw materials for the conventional layer: 75 parts of linear polyethylene resin, 24 parts of low-density polyethylene, and 1 part of anti-blocking masterbatch.
[0046] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0047] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0048] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 35.2N / 5cm, a MD breaking strength of 64.6N / 5cm, and a surface resistance of 9.8×10 10 Ω.
[0049] After the antistatic PE film is heat-sealed with the antistatic PE film, the heat-sealed part is not damaged and can be easily torn after being torn. After the antistatic PE film is heat-sealed with the 50μm conventional 100% PE, the heat-sealed part is not damaged and can be easily torn after being torn.
[0050] Example 3
[0051] The raw materials of the antistatic heat-sealing layer: 44 parts of linear polyethylene resin, 22 parts of low-density polyethylene, 15 parts of 1-butene-based polymer, 10 parts of EVA resin, 7 parts of antistatic masterbatch, and 2 parts of anti-adhesion masterbatch; the raw materials of the conventional layer: 57 parts of linear polyethylene resin, 41 parts of low-density polyethylene, and 2 parts of anti-adhesion masterbatch.
[0052] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0053] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0054] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 30.4N / 5cm, a MD breaking strength of 58.3N / 5cm, and a surface resistance of 5.8×10 10 Ω.
[0055] After the antistatic PE film is heat-sealed with the antistatic PE film, the heat-sealed part is not damaged and can be easily torn after being torn. After the antistatic PE film is heat-sealed with the 50μm conventional 100% PE, the heat-sealed part is not damaged and can be easily torn after being torn.
[0056] Example 4
[0057] The raw materials of the antistatic heat-sealing layer: 40 parts of linear polyethylene resin, 21 parts of low-density polyethylene, 20 parts of 1-butene-based polymer, 6 parts of EVA resin, 10 parts of antistatic masterbatch, 3 parts of anti-adhesion masterbatch; the raw materials of the conventional layer: 50 parts of linear polyethylene resin, 48 parts of low-density polyethylene, and 2 parts of anti-adhesion masterbatch.
[0058] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0059] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0060] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 28.5N / 5cm, a MD breaking strength of 54.1N / 5cm, and a surface resistance of 1.3×10 10 Ω.
[0061] After the antistatic PE film is heat-sealed with the antistatic PE film, the heat-sealed part is not damaged after tearing and is easy to tear. After the antistatic PE film is heat-sealed with 50μm conventional 100% PE, the heat-sealed part is not damaged after tearing and is easy to tear.
[0062] Comparative Example 1
[0063] The raw materials of the antistatic heat-sealing layer: 60 parts of linear polyethylene resin, 21 parts of low-density polyethylene, 27 parts of 1-butene-based polymer, 10 parts of antistatic masterbatch, 3 parts of anti-blocking masterbatch; the raw materials of the conventional layer: 50 parts of linear polyethylene resin, 48 parts of low-density polyethylene, and 2 parts of anti-blocking masterbatch.
[0064] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0065] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0066] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 33.2N / 5cm, a MD breaking strength of 60.2N / 5cm, and a surface resistance of 1.3×10 10 Ω.
[0067] After the antistatic PE film is heat-sealed with itself, the heat-sealed part is damaged and difficult to tear after tearing. After the antistatic PE film is heat-sealed with 50μm conventional 100% PE, the heat-sealed part is damaged and difficult to tear after tearing.
[0068] Comparative Example 2
[0069] The raw materials of the antistatic heat-sealing layer: 50 parts of linear polyethylene resin, 25 parts of low-density polyethylene, 15 parts of 1-butene-based polymer, 8 parts of antistatic masterbatch, 2 parts of anti-blocking masterbatch; the raw materials of the conventional layer: 50 parts of linear polyethylene resin, 48 parts of low-density polyethylene, 2 parts of anti-blocking masterbatch.
[0070] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0071] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0072] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 60.2N / 5cm, a MD breaking strength of 59.5N / 5cm, and a surface resistance of 5.3×10 10 Ω.
[0073] After the antistatic PE film is heat-sealed with itself, the heat-sealed part is slightly damaged after tearing and can be easily torn. After the antistatic PE film is heat-sealed with 50μm conventional 100% PE, the heat-sealed part is damaged in varying sizes after tearing and can be easily torn.
[0074] Comparative Example 3
[0075] The raw materials of the antistatic heat-sealing layer: 50 parts of linear polyethylene resin, 25 parts of low-density polyethylene, 15 parts of EVA resin, 8 parts of antistatic masterbatch, 2 parts of anti-adhesion masterbatch; the raw materials of the conventional layer: 50 parts of linear polyethylene resin, 48 parts of low-density polyethylene, 2 parts of anti-adhesion masterbatch.
[0076] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0077] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0078] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 29.2N / 5cm, a MD breaking strength of 58.1N / 5cm, and a surface resistance of 5.5×10 10 Ω.
[0079] After the antistatic PE film is heat-sealed to itself, the heat-sealed part is damaged after tearing and is generally easy to tear. After the antistatic PE film is heat-sealed to 50μm conventional 100% PE, the heat-sealed part is damaged after tearing and is generally easy to tear.
[0080] Comparative Example 4
[0081] The raw materials of the antistatic heat-sealing layer: 50 parts of linear polyethylene resin, 25 parts of low-density polyethylene, 15 parts of EVA resin, 8 parts of antistatic masterbatch, 2 parts of anti-blocking masterbatch; the raw materials of the conventional layer: 42 parts of linear polyethylene resin, 20 parts of low-density polyethylene, 20 parts of 1-butene-based polymer, 15 parts of EVA resin, 3 parts of anti-blocking masterbatch.
[0082] The raw materials of the antistatic heat-sealing layer and the raw materials of the conventional layer were placed in two heating mixers respectively, and stirred and dried for 35 minutes at 70°C.
[0083] Add the antistatic heat-sealing layer raw materials into the two outermost screw barrels of the film blowing machine, and add the conventional layer raw materials into the middle screw barrel. After being plasticized and melted by the screw in the extruder, the molten raw materials are finally transported to the die mouth for blowing and cooling under the pressure and forward thrust of the screw. The outermost layer is the antistatic heat-sealing layer, and the middle is the conventional layer. The screw temperature is 105℃~155℃; the die head temperature of the casting machine is 130℃~160℃; the thickness of the formed film is 50 microns, and the winding speed is 60m / min.
[0084] The antistatic PE film obtained above has a transparent and soft appearance, a CD breaking strength of 28.1 N / 5 cm, an MD breaking strength of 56.1 N / 5 cm, and a surface resistance of 4.1×1010Ω.
[0085] After the antistatic PE film is heat-sealed with itself, the heat-sealed part is damaged and can be easily torn after being torn. After the antistatic PE film is heat-sealed with 50μm conventional 100% PE, the heat-sealed part is damaged and can be easily torn after being torn.
[0086] In the performance tests of the above Examples 1 to 4 and Comparative Examples 1 to 4, the breaking strength was tested according to the ISO9073-3 method, and the antistatic was tested according to the EN1149-1 method.
[0087] From the comparison of the test results, it can be seen that the blown films of Examples 1 to 4 of the present invention have excellent antistatic properties, breaking strength, and tearability after heat sealing. The breaking strength can reach at least 25.5N / 5cm, and the surface resistance is at most 9.8×10 10 Ω, good antistatic property, can meet the requirements of medical protection antistatic property and tearability after heat sealing, and the preparation process is stable.
[0088] From the results of Examples 1 to 4 and Comparative Examples 1 to 4, it can be seen that in the production process of the antistatic film, the outer layer raw materials 1-butene-based polymer resin, EVA resin and PE (polyethylene) are blended and added to a screw, and they are heat-sealed with themselves or with 100% PE, and they have good tearability after heat-sealing. When only one 1-butene-based polymer resin or EVA resin is added to the outer layer raw material, the inner layer does not have general tearability after heat-sealing even if it is a heat-sealing formula.
[0089] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A tearable antistatic film, characterized in that: It comprises a conventional layer and an antistatic heat-sealing layer integrally compounded on opposite sides of the conventional layer; The conventional layer includes the following raw materials and their weight proportions: 40-75 parts of linear polyethylene, 24-57 parts of low-density polyethylene and 1-3 parts of anti-blocking masterbatch; The antistatic heat-sealing layer includes raw materials and their mass proportions are as follows: 26-62 parts of linear polyethylene, 16-26 parts of low-density polyethylene, 10-20 parts of 1-butene-based polymer, 6-15 parts of EVA resin, 5-10 parts of antistatic masterbatch and 1-3 parts of anti-adhesion masterbatch.
2. The tearable antistatic film according to claim 1, characterized in that: The density of the linear polyethylene is 0.91 g / cm 3 ~0.94g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.2g / 10min to 2.5g / 10min.
3. The tearable antistatic film according to claim 1, characterized in that: The density of the low-density polyethylene is 0.91 g / cm 3 ~0.925g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 1.7 g / 10min to 2.3 g / 10min.
4. The tearable antistatic film according to claim 1, characterized in that: The density of the 1-butene-based polymer is 0.91 g / cm 3 ~0.93g / cm 3 The melt index is 3g / 10min~4g / 10min at a temperature of 190°C and a load of 2160g.
5. The tearable antistatic film according to claim 1, characterized in that: The density of the EVA resin is 0.92 g / cm 3 ~0.95g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 2g / 10min to 3g / 10min.
6. The tearable antistatic film according to claim 1, characterized in that: The density of the antistatic masterbatch is 0.93 g / cm 3 The melt index at a temperature of 190°C and a load of 2160 g is 6 g / 10 min.
7. The tearable antistatic film according to claim 1, characterized in that: The density of the anti-adhesion masterbatch is 1g / cm 3 ~1.2g / cm 3 The melt index at a temperature of 190°C and a load of 2160g is 6g / 10min to 9g / 10min.
8. The tearable antistatic film according to any one of claims 1 to 7, characterized in that: The tearable antistatic film has a thickness of 30 μm to 200 μm; The thickness ratio of the antistatic heat-sealing layer on one side of the conventional layer to the conventional layer is 0.8-1.5:
1.
9. A method for preparing a tearable antistatic film according to any one of claims 1 to 8, characterized in that: The following steps are involved: The raw materials of the conventional layer and the antistatic heat-sealing layer are heated, stirred and dried respectively, and then sent to the barrel of the film blowing machine, and co-extruded and blown by the extruder to form a composite tearable antistatic film, which is then cooled, shaped, pulled, slit and rolled.
10. Use of the tearable antistatic film according to any one of claims 1 to 8, characterized in that: Used for medical drapes or isolation gowns.
Citation Information
Patent Citations
Biaxially-oriented polyethylene shrink film and production technique thereof
CN102774110A
Film with characteristic of easy tearing in longitudinal direction, and preparation method thereof
CN107629281A