Lithium sulfide and preparation method thereof
By co-precipitation reaction of lithium chloride and ammonium sulfide in the protective gas atmosphere, the problems of highly toxic gases and high-temperature treatment in the existing lithium sulfide preparation are solved, and the low-cost preparation and simple treatment of high-purity lithium sulfide are achieved. Have industrial application prospects.
Patent Information
- Application Number
- CN202411047765.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-08
AI Technical Summary
The existing lithium sulfide preparation methods have safety risks brought about by the use of highly toxic gases, high energy consumption costs caused by high temperature treatment, complex purification steps and high waste gas treatment costs, which hinder the industrial promotion of lithium sulfide.
The co-precipitation reaction is carried out by mixing lithium chloride and ammonium sulfide in a protective gas atmosphere to obtain lithium sulfide and obtain a high-purity product through drying. At the same time, the by-product ammonium chloride is recovered, avoiding highly toxic gases and high-temperature treatment.
It realizes high safety preparation of lithium sulfide, reduces production costs, simplifies subsequent processing processes, and has industrial application prospects.
Smart Images

Figure BDA0004973979110000091 
Figure BDA0004973979110000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a method for preparing lithium sulfide, in particular to lithium sulfide and a method for preparing the same. Background Art
[0002] As a key material, lithium sulfide plays an important role in the field of solid-state batteries. Solid electrolytes are the core components of solid-state batteries, and lithium sulfide, as a key raw material for synthesizing sulfide solid electrolytes, is crucial to improving the performance of solid-state batteries. At the same time, lithium sulfide is also considered to be a promising pre-lithiation agent that can make up for the problem of irreversible lithium loss in the first cycle of lithium-ion batteries and improve the energy density and cycle stability of batteries.
[0003] CN112624060A discloses the use of industrial-grade butyl lithium to prepare high-purity lithium sulfide, taking lithium chloride, industrial-grade n-butyl lithium solution and n-hexane to fully mix to obtain a mixed solution, then introducing H2S gas to obtain a reaction slurry, and filtering to obtain a crude lithium sulfide solid wet material. The document uses industrial-grade butyl lithium to prepare high-purity lithium sulfide, which has the advantages of simple process and high yield. However, it is necessary to use highly toxic gas hydrogen sulfide, which will bring great safety risks and subsequent high-temperature treatment is required, which also increases energy consumption costs.
[0004] CN117550562A discloses that lithium hydroxide and sulfur powder are mixed and ground, and then mixed with hydrazine hydrate to obtain lithium sulfide slurry; the lithium sulfide slurry is heated and dried, and then sulfur powder and anhydrous hydrazine are added, and the temperature is again raised to dryness to obtain high-purity lithium sulfide powder. Although this document prepares high-purity lithium sulfide by a one-pot method, materials such as hydrazine hydrate and anhydrous hydrazine are strictly controlled hazardous chemicals and react to generate highly toxic gas hydrogen sulfide, which increases the cost of tail gas treatment.
[0005] CN115535969A discloses weighing anhydrous lithium salt and sodium sulfide and mixing them, reacting the two raw materials in a polar solvent; collecting the solid phase product after solid-liquid separation; washing the solid phase product with a weak polar solvent, and then drying to obtain a crude lithium sulfide product; and finally calcining to obtain a fine lithium sulfide product. The product prepared by this method has high purity, no greenhouse gas emissions, by-products can be collected, and auxiliary solvents can be recycled and reused. However, the purification steps of the product are relatively complicated, which is not conducive to industrialization.
[0006] The preparation methods of lithium sulfide disclosed in the prior art all have certain defects, such as high risks due to the use of toxic gases, high costs due to the need for high-temperature treatment, high waste gas treatment costs due to the generation of toxic tail gas, and complex product purification steps that are not conducive to industrial promotion. The high production cost also hinders the expansion of lithium sulfide production capacity. Therefore, it is urgent to develop a new method for preparing lithium sulfide. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a lithium sulfide and a preparation method thereof. The lithium sulfide preparation method provided by the present invention does not use highly toxic raw materials, the reaction conditions are mild, and the coprecipitation reaction does not produce toxic substances. High-purity lithium sulfide can be obtained by drying only. Therefore, the preparation method has the advantages of high safety, low preparation cost and simple post-processing process, and has industrial application prospects. In addition, the preparation method can also obtain ammonium chloride as a byproduct with added value.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a method for preparing lithium sulfide, the preparation method comprising:
[0010] In a protective gas atmosphere, lithium chloride, ammonium sulfide and an organic solvent are mixed to obtain lithium sulfide and an organic solution containing ammonium chloride through a co-precipitation reaction.
[0011] The chemical equation of the coprecipitation reaction in the present invention is: 2LiCl+(NH4)2S=Li2S+2NH4Cl.
[0012] The preparation method of lithium sulfide provided by the present invention does not use highly toxic raw materials, the reaction conditions are mild, and the reaction does not produce toxic substances. High-purity lithium sulfide can be obtained by drying only. Therefore, the preparation method has the advantages of high safety, low preparation cost and simple post-processing process, and has industrial application prospects. In addition, the preparation method can also obtain ammonium chloride as a byproduct with added value.
[0013] Preferably, the molar ratio of lithium chloride to ammonium sulfide is (1.8-2.3):1, for example, it can be 1.8:1, 1.85:1, 1.9:1, 1.95:1, 2:1, 2.05:1, 2.1:1, 2.15:1, 2.2:1, 2.25:1 or 2.3:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] Preferably, the molar ratio of the lithium chloride to the organic solvent is 1:(2-5), for example, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, 1:2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the organic solvent comprises any one of dimethyl sulfoxide, dimethylamide, N-methylpyrrolidone or sulfolane, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of dimethyl sulfoxide and dimethyl sulfoxide, a combination of dimethyl sulfoxide and N-methylpyrrolidone, a combination of N-methylpyrrolidone and sulfolane, or a combination of dimethyl sulfoxide, dimethyl sulfoxide, N-methylpyrrolidone and sulfolane.
[0016] Preferably, the mixing comprises: completely dissolving lithium chloride in an organic solvent to obtain a lithium chloride organic solution, and then adding ammonium sulfide.
[0017] Preferably, the mixing and dissolving process is accompanied by stirring.
[0018] Preferably, the coprecipitation reaction is carried out at a temperature of 20 to 40° C. and for a time of 4 to 8 hours.
[0019] The temperature of the coprecipitation reaction in the present invention is 20-40°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C or 40°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] The coprecipitation reaction time in the present invention is 4 to 8 hours, for example, it can be 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the coprecipitation reaction is accompanied by stirring.
[0022] Preferably, the preparation method further comprises solid-liquid separation after the coprecipitation reaction to obtain crude lithium sulfide and an organic solution containing ammonium chloride, and drying the obtained crude lithium sulfide in a protective gas atmosphere to obtain lithium sulfide.
[0023] In the present invention, high-purity lithium sulfide can be obtained by drying the obtained crude lithium sulfide in a protective gas atmosphere, and the purification method is simple and effective.
[0024] Preferably, the solid-liquid separation method includes centrifugation or filtration.
[0025] Preferably, the drying temperature is 150-200° C. and the drying time is 2-4 hours.
[0026] The drying temperature in the present invention is 150-200°C, for example, it can be 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] The drying time described in the present invention is 2 to 4 hours, for example, it can be 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours or 4 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the preparation method further comprises fractionating the organic solution containing ammonium chloride, and absorbing the distilled ammonium chloride gas by water to obtain the ammonium chloride solution and the organic solvent.
[0029] In the present invention, by fractionating the organic solution containing ammonium chloride, ammonium chloride with added value can be obtained, and the recovery of the organic solvent is achieved. The recovered organic solvent can be used in the preparation method of the present invention to prepare lithium sulfide again.
[0030] Preferably, the fractionation temperature is 100-150° C. and the time is 2-6 hours.
[0031] The distillation temperature in the present invention is 100-150°C, for example, it can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C or 150°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] The distillation time in the present invention is 2 to 6 hours, for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises:
[0034] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:(2-5), and the molar ratio of the lithium chloride to the ammonium sulfide is (1.8-2.3):1, and after a coprecipitation reaction at 20-40° C. for 4-8 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0035] (2) drying the crude lithium sulfide obtained in step (1) at 150-200° C. for 2-4 hours in a protective gas atmosphere to obtain finished lithium sulfide;
[0036] (3) fractionating the organic solution containing ammonium chloride obtained in step (1) at 100-150° C. for 2-6 hours, and absorbing the distilled ammonium chloride gas with water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is reused in step (1).
[0037] In a second aspect, the present invention provides a lithium sulfide, which is obtained by the preparation method described in the first aspect.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The preparation method of lithium sulfide provided by the present invention uses relatively low-cost lithium chloride and ammonium sulfide as raw materials, and does not use toxic gases; reacts at low temperature and normal pressure, and filters to obtain crude lithium sulfide and an organic solution containing ammonium chloride. No polluting gas is generated during the reaction process, and the crude lithium sulfide is dried under an inert gas atmosphere to obtain a high-purity product. Therefore, the preparation method has the advantages of high safety, mild reaction conditions, simple purification process, and no pollutants. In addition, the preparation method can also obtain the by-product ammonium chloride with added value, and the organic solvent can also be reused in the preparation method of the present invention to prepare lithium sulfide again. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0041] Example 1
[0042] This embodiment provides a method for preparing lithium sulfide, the preparation method comprising:
[0043] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:3, and the molar ratio of the lithium chloride to the ammonium sulfide is 2:1, and after a coprecipitation reaction at 30° C. for 6 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0044] (2) drying the crude lithium sulfide obtained in step (1) at 180° C. for 3 h in a protective gas atmosphere to obtain finished lithium sulfide;
[0045] (3) The organic solution containing ammonium chloride obtained in step (1) is fractionated at 130° C. for 4 hours, and the distilled ammonium chloride gas is absorbed by water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
[0046] Example 2
[0047] This embodiment provides a method for preparing lithium sulfide, the preparation method comprising:
[0048] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:2, and the molar ratio of the lithium chloride to the ammonium sulfide is 1.9:1, and after a coprecipitation reaction at 35° C. for 5 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0049] (2) drying the crude lithium sulfide obtained in step (1) at 190° C. for 2.5 hours in a protective gas atmosphere to obtain finished lithium sulfide;
[0050] (3) The organic solution containing ammonium chloride obtained in step (1) is fractionated at 150° C. for 2 h, and the distilled ammonium chloride gas is absorbed by water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
[0051] Example 3
[0052] This embodiment provides a method for preparing lithium sulfide, the preparation method comprising:
[0053] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:5, and the molar ratio of the lithium chloride to the ammonium sulfide is 2.1:1, and after a coprecipitation reaction at 25° C. for 7 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0054] (2) drying the crude lithium sulfide obtained in step (1) at 150° C. for 4 hours in a protective gas atmosphere to obtain finished lithium sulfide;
[0055] (3) The organic solution containing ammonium chloride obtained in step (1) is fractionated at 140° C. for 3 h, and the distilled ammonium chloride gas is absorbed by water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
[0056] Example 4
[0057] This embodiment provides a method for preparing lithium sulfide, the preparation method comprising:
[0058] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:2.5, and the molar ratio of the lithium chloride to the ammonium sulfide is 2.3:1, and after a coprecipitation reaction at 20° C. for 8 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0059] (2) drying the crude lithium sulfide obtained in step (1) at 200° C. for 2 h in a protective gas atmosphere to obtain finished lithium sulfide;
[0060] (3) The organic solution containing ammonium chloride obtained in step (1) is fractionated at 100° C. for 6 hours, and the distilled ammonium chloride gas is absorbed by water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
[0061] Example 5
[0062] This embodiment provides a method for preparing lithium sulfide, the preparation method comprising:
[0063] (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent, and then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:4, and the molar ratio of the lithium chloride to the ammonium sulfide is 1.8:1, and after a coprecipitation reaction at 40° C. for 4 hours, solid-liquid separation is performed to obtain a crude lithium sulfide and an organic solution containing ammonium chloride;
[0064] (2) drying the crude lithium sulfide obtained in step (1) at 165° C. for 3.5 hours in a protective gas atmosphere to obtain finished lithium sulfide;
[0065] (3) The organic solution containing ammonium chloride obtained in step (1) is fractionated at 115° C. for 5 hours, and the distilled ammonium chloride gas is absorbed by water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
[0066] Example 6
[0067] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the molar ratio of lithium chloride to ammonium sulfide in step (1) is 1.5:1.
[0068] Example 7
[0069] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the molar ratio of lithium chloride to ammonium sulfide in step (1) is 2.5:1.
[0070] Example 8
[0071] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the molar ratio of lithium chloride to organic solvent in step (1) is 1:1.5.
[0072] Example 9
[0073] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the molar ratio of lithium chloride to organic solvent in step (1) is 1:6.
[0074] Example 10
[0075] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the temperature of the coprecipitation reaction in step (1) is 10°C.
[0076] Embodiment 11
[0077] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the temperature of the coprecipitation reaction in step (1) is 50°C.
[0078] Example 12
[0079] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the drying temperature in step (2) is 130°C.
[0080] Embodiment 13
[0081] This embodiment provides a method for preparing lithium sulfide, which is the same as that of Embodiment 1 except that the drying temperature in step (2) is 240°C.
[0082] Comparative Example 1
[0083] This comparative example provides a method for preparing lithium sulfide, which is the same as Example 1 except that lithium chloride is replaced by lithium nitrate having the same molar amount of lithium.
[0084] Comparative Example 2
[0085] This comparative example provides a method for preparing lithium sulfide, which is the same as Example 1 except that ammonium sulfide is replaced by hydrogen sulfide with the same molar amount of sulfur.
[0086] Lithium sulfide was prepared by the preparation method of lithium sulfide provided in the above embodiment and comparative example, and the obtained lithium sulfide was subjected to ICP detection. The purity of the lithium sulfide was measured by reduction method. The results are shown in Table 1.
[0087] Table 1
[0088]
[0089]
[0090] From Table 1, we can get:
[0091] (1) The preparation method of lithium sulfide provided in Examples 1 to 5 of the present invention does not use highly toxic raw materials, the reaction conditions are mild, and no toxic substances are produced after the reaction. High-purity lithium sulfide can be obtained by drying only. Therefore, the preparation method has the advantages of high safety, low preparation cost and simple post-processing process, and has the prospect of industrial application; in addition, the preparation method can also obtain ammonium chloride as a byproduct with added value;
[0092] (2) By comparing Example 1 with Examples 6 and 7, it can be seen that the molar ratio of lithium chloride to ammonium sulfide in the present invention will affect the purity of the prepared lithium sulfide; when the molar ratio of lithium chloride to ammonium sulfide is low, the purity of the lithium sulfide will be low, because insufficient lithium chloride will cause the ammonium sulfide to fail to react completely, and the residual ammonium sulfide may be wrapped by lithium sulfide, resulting in unreacted ammonium sulfide mixed in the precipitate, thereby reducing the purity of the lithium sulfide; when the molar ratio of lithium chloride to ammonium sulfide is high, the purity of the lithium sulfide will be low, because the high molar ratio will increase the concentration of lithium chloride in the reaction system, thereby increasing the risk of unreacted lithium chloride remaining in the lithium sulfide, and excessive lithium chloride will affect the growth of lithium sulfide crystals, resulting in smaller crystal size, increased surface area, and increased possibility of impurity adsorption;
[0093] (3) By comparing Example 1 with Examples 8 and 9, it can be seen that the molar ratio of lithium chloride to organic solvent in the present invention affects the purity of the prepared lithium sulfide; when the molar ratio of lithium chloride to organic solvent is low, the purity of lithium sulfide will be low, because too much solvent will dilute the concentration of the reactants, reduce the collision probability of the reactants, and thus slow down the reaction rate; when the molar ratio of lithium chloride to organic solvent is high, the purity of lithium sulfide will be low, because too little solvent may limit the diffusion of the reactants, resulting in uneven heat transfer in the system, causing local overheating or overcooling of the reaction system, affecting the reaction efficiency;
[0094] (4) By comparing Example 1 with Examples 10 and 11, it can be seen that the temperature of the coprecipitation reaction in the present invention will affect the purity of the prepared lithium sulfide; when the temperature of the coprecipitation reaction is low, the purity of the lithium sulfide will be low. This is because when the temperature is too low, it is not conducive to the growth of lithium sulfide crystals, resulting in small lithium sulfide particles and incomplete crystallization, which increases the possibility of impurity adsorption. Moreover, when the temperature is too low, it will affect the stability of the precipitation, making the precipitation easy to aggregate or form agglomerates, thereby causing the lithium sulfide to wrap more impurities; when the temperature of the coprecipitation reaction is high, the purity of the lithium sulfide will be low. This is because when the temperature is too high, the rate of the coprecipitation reaction will be too fast, resulting in impurity coating; at the same time, too high a temperature will also affect the crystal structure of lithium sulfide, resulting in an increase in crystal defects and an increase in the possibility of impurity adsorption, thereby causing the purity of the lithium sulfide to be low;
[0095] (5) By comparing Example 1 with Examples 12 and 13, it can be seen that the temperature at which the crude lithium sulfide is dried in the present invention affects the purity of the prepared lithium sulfide; when the drying temperature is low, the purity of the lithium sulfide is low, because too low a drying temperature will lead to incomplete drying, and impurities such as organic solvents on the surface cannot be completely removed, thereby affecting the purity of the lithium sulfide; when the drying temperature is high, the purity of the lithium sulfide is low, because too high a drying temperature may cause the residual solvent to react with the lithium sulfide to generate new impurities, resulting in reduced purity;
[0096] (6) By comparing Example 1 with Comparative Example 1, it can be seen that if lithium chloride is replaced with lithium nitrate having the same molar amount of lithium, the purity of lithium sulfide will be lower. This is because lithium nitrate will not react with ammonium sulfide as quickly and completely as lithium chloride, resulting in incomplete reaction, thereby affecting the purity;
[0097] (7) By comparing Example 1 with Comparative Example 2, it can be seen that if ammonium sulfide is replaced by hydrogen sulfide with the same molar amount of sulfur, the purity of lithium sulfide will be low. This is because hydrogen sulfide has a low solubility in organic solvents and is difficult to effectively react with lithium chloride to form lithium sulfide at conventional temperatures and pressures. In addition, hydrogen sulfide may react with organic solvents to form by-products such as sulfur or polysulfides, which may be mixed into lithium sulfide. In addition, hydrogen sulfide may react with lithium chloride to form other sulfides, thereby affecting the purity of lithium sulfide. Furthermore, since hydrogen sulfide is a toxic gas, it will also reduce the safety of the reaction.
[0098] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing lithium sulfide, characterized in that: The preparation method comprises: In a protective gas atmosphere, lithium chloride, ammonium sulfide and an organic solvent are mixed to obtain lithium sulfide and an organic solution containing ammonium chloride through a co-precipitation reaction.
2. The preparation method according to claim 1, characterized in that: The molar ratio of lithium chloride to ammonium sulfide is (1.8-2.3):1; Preferably, the molar ratio of the lithium chloride to the organic solvent is 1:(2-5).
3. The preparation method according to claim 1 or 2, characterized in that: The organic solvent includes any one of dimethyl sulfoxide, dimethylamide, N-methylpyrrolidone or sulfolane, or a combination of at least two thereof.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The mixing comprises: lithium chloride is completely dissolved in an organic solvent to obtain a lithium chloride organic solution, and then ammonium sulfide is added.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The coprecipitation reaction is carried out at a temperature of 20 to 40° C. and for a time of 4 to 8 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The preparation method further comprises solid-liquid separation after the coprecipitation reaction to obtain crude lithium sulfide and an organic solution containing ammonium chloride, and drying the obtained crude lithium sulfide in a protective gas atmosphere to obtain lithium sulfide; Preferably, the drying temperature is 150-200° C. and the drying time is 2-4 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method further comprises fractionating an organic solution containing ammonium chloride, and absorbing the fractionated ammonium chloride gas by water to obtain an ammonium chloride solution and an organic solvent.
8. The preparation method according to claim 7, characterized in that: The fractionation temperature is 100-150° C. and the distillation time is 2-6 hours.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method comprises: (1) in a protective gas atmosphere, completely dissolving lithium chloride in an organic solvent to obtain a lithium chloride organic solution, then adding ammonium sulfide, wherein the molar ratio of the lithium chloride to the organic solvent is 1:(2-5), and the molar ratio of the lithium chloride to the ammonium sulfide is (1.8-2.3):1, performing a coprecipitation reaction at 20-40° C. for 4-8 hours, and performing solid-liquid separation to obtain a crude lithium sulfide and an organic solution containing ammonium chloride; (2) drying the crude lithium sulfide obtained in step (1) at 150-200° C. for 2-4 hours in a protective gas atmosphere to obtain finished lithium sulfide; (3) fractionating the organic solution containing ammonium chloride obtained in step (1) at 100 to 150° C. for 2 to 6 hours, and absorbing the distilled ammonium chloride gas with water to obtain an ammonium chloride solution and an organic solvent, and the obtained organic solvent is used in step (1).
10. A lithium sulfide, characterized in that: The lithium sulfide is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Liquid phase precipitation method for preparing lithium sulfide and lithium sulfide
CN115535969A
Method of making anhydrous metal sulfide nanocrystals
US20210261411A1
Lithium sulfide production method
US20230150818A1
Cited By
Method for preparing lithium sulfide through high-temperature solid-phase reaction
CN120097284A
Lithium sulfide and method for preparing lithium sulfide
CN120589692A
Lithium sulfide and a method of producing lithium sulfide
CN120589692B
Preparation method of high-purity lithium sulfide
CN122561842A