Preparation method and application of nano vanadium sodium fluorophosphate positive electrode material
Nano-Vanulium Vanadium Fluorophosphate was synthesized by solvent thermal method and in situ carbon coating, which solved the problem of particle breakage caused by low electronic conductivity and volume changes of vanadium Vanadium Fluorophosphate, and improved the electrochemical performance and cycle stability of the material. In the field of energy storage of sodium ion batteries.
Patent Information
- Application Number
- CN202410997618.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
As the positive electrode material of the battery, sodium vanadium fluorophosphate has the problem of low electron conductivity and large volume changes, resulting in the breaking and falling off of particles. In addition, decomposition side reactions are prone to occur at high temperatures in solid phase synthesis, affecting the electrochemical performance and application pace of the material.
The nano-vinyl vanadium fluorophosphate was synthesized by solvothermal method and coated by in-situ carbon to shorten the electron and ion transmission distance, improve the electron conductivity of the material surface, avoid side reactions of decomposition at high temperatures, and generate a pure single-crystal material.
It significantly improves the capacity, magnification and circulation performance of the material, ensures the uniformity of the material and the consistency of multiple batches, extends the cycle life, and avoids particle breakage and shedding.
Smart Images

Figure CN118908174A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a preparation method and application of a nano sodium vanadium fluorophosphate positive electrode material. Background Art
[0002] New green energy is the top priority of future energy development. Solar energy, wind energy, and tidal energy in new energy sources have uncertain and intermittent production capacity, which makes it difficult to access the grid. Therefore, it is necessary to develop large-scale energy storage equipment that is used in conjunction with new green energy. Lithium-ion batteries have been widely used in portable electronic devices, electric vehicles, large-scale energy storage equipment, and other fields due to their high energy density, high power density, long cycle life, and no memory effect. In recent years, with the explosive growth of electric vehicles, the price of Li2CO3, the basic material of lithium-ion batteries, has continued to rise, and the price of lithium-ion batteries has remained high. The extremely low cost performance makes it difficult to use them in the field of large-scale energy storage equipment.
[0003] Sodium-ion batteries have similar battery structures and charging and discharging principles to lithium-ion batteries. Sodium and lithium belong to the first main group of alkali metal elements and have similar physical and chemical properties. However, the storage capacity of sodium in the earth's crust can reach 2.83%, which is much higher than that of lithium (0.0065%). It has the advantages of wide distribution and low price. At the same time, sodium-ion batteries have higher safety, low-temperature performance and power characteristics. These advantages make sodium-ion batteries have good application prospects in the fields of cost-effective low-speed electric vehicles, power tools and energy storage.
[0004] Sodium vanadium fluorophosphate has a stable three-dimensional open framework structure that allows ions to be reversibly embedded and deintercalated in three directions with little change in the volume of the structure. It has a high theoretical capacity and operating voltage and is considered to be one of the best choices for battery cathode materials in the field of energy storage. However, due to the low electronic conductivity of sodium vanadium fluorophosphate and the volume change during the charge and discharge process that causes particle breakage and shedding, and the fact that solid-phase synthesis of materials is prone to decomposition side reactions at high temperatures, resulting in significant deviations in material consistency, these problems have seriously affected the electrochemical performance and application of the material. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method for preparing a nano sodium vanadium fluorophosphate positive electrode material and its application. The material improves the problem of poor intrinsic electronic conductivity of sodium vanadium fluorophosphate and large volume change during the cycle, which leads to particle breakage and shedding, by in-situ carbon coating and material nano-materialization, and effectively improves the capacity, rate and cycle performance of the material. In addition, the solvothermal method can effectively avoid the uneven temperature range of the material at high temperature during the sol-gel and solid-phase synthesis process, which leads to decomposition to form a sodium vanadium phosphate impurity phase, as well as the phenomenon of partial fluorine-position oxygen doping, and directly generates a pure phase single crystal sodium vanadium fluorophosphate positive electrode material, effectively ensuring the uniformity of material synthesis and consistency of multiple batches.
[0006] The scheme of the present invention is:
[0007] A method for preparing a nano sodium vanadium fluorophosphate positive electrode material comprises the following steps:
[0008] 1) taking a sodium source, a vanadium source, a fluorine source and a phosphorus source respectively according to the element molar ratio of Na:V:P:F=x:2:2:3, and taking a carbon source, wherein 3<x<6;
[0009] 2) adding the vanadium source, sodium source, fluorine source and carbon source in 1) into the inner lining of the hydrothermal reactor in sequence, and then adding the organic solvent and phosphorus source, stirring and mixing evenly; wherein the carbon source is used as carbon coating on the surface of the material;
[0010] 3) transferring the mixed solution in the lining of the hydrothermal kettle in 2) to the hydrothermal kettle, heating it to 120-250° C., keeping the temperature constant for 1-50 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder, namely Na3V2(PO4)2F3;
[0011] 4) The sodium vanadium fluorophosphate powder obtained in 3) is heated to 400-800° C. at a heating rate of 1-10° C. / min under an inert atmosphere, kept at a constant temperature for 0.1-10 h, and then naturally cooled to room temperature to obtain a carbon-coated nano sodium vanadium fluorophosphate positive electrode material.
[0012] As a preferred technical solution, the vanadium source in 1) is one or more of ammonium metavanadate, vanadium pentoxide, vanadium trichloride, vanadium tribromide, vanadium trioxide, vanadium acetylacetonate and vanadyl sulfate; the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and ammonium phosphate; the carbon source is formic acid (HCOOH), gallic acid (C7H6O5·H2O), oxalic acid (H2C2O4·2H2O), tartaric acid (C4H6O6), malic acid (C4H6O5), citric acid (C6H8O7·H2O) and EDTA (C 10 H 16 N2O8), wherein the amount of carbon in the carbon source is 150-300% of the molar number of vanadium.
[0013] As a preferred technical solution, the sodium source in 2) is one or more of sodium fluoride, sodium chloride, sodium carbonate, sodium hydroxide, sodium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium citrate, sodium oxalate, sodium phosphate and sodium nitrate; the fluorine source is one or more of sodium fluoride, ammonium fluoride, potassium fluoride and magnesium fluoride.
[0014] As a preferred technical solution, the organic solvent in 2) is one or more of methanol, ethanol, ethylene glycol, ethylenediamine, acetonitrile, acetone, nitromethane, dimethylformamide, triethylamine, dimethyl sulfoxide, butyrolactone and propylene carbonate, and the amount of the solvent is 60% of the volume of the hydrothermal autoclave.
[0015] As a preferred technical solution, in the step 2), the stirring speed is 100 to 800 r / min, the stirring temperature is 10 to 100° C., and the stirring time is 0.1 to 2 h.
[0016] As a preferred technical solution, the inert atmosphere in 4) is one or more of argon, argon-hydrogen mixed gas and nitrogen.
[0017] The invention also discloses a carbon-coated nano sodium vanadium fluorophosphate positive electrode material prepared by a method for preparing the nano sodium vanadium fluorophosphate positive electrode material.
[0018] As a preferred technical solution, the carbon-coated nano sodium vanadium fluorophosphate positive electrode material is a structure formed by agglomeration of amorphous carbon-coated nano-sheet sodium vanadium fluorophosphate primary particles.
[0019] The invention also discloses the application of a carbon-coated nano sodium vanadium fluorophosphate positive electrode material in a sodium ion battery.
[0020] Due to the adoption of the above technical scheme, a method for preparing a nano sodium vanadium fluorophosphate positive electrode material comprises the following steps: 1) taking a sodium source, a vanadium source, a fluorine source and a phosphorus source respectively according to the element ratio Na:V:P:F=x:2:2:3, and taking a carbon source, wherein 3<x<6; 2) adding the vanadium source, the sodium source, the fluorine source and the carbon source in 1) into the lining of a hydrothermal kettle in sequence, then adding an organic solvent and a phosphorus source, and stirring and mixing them uniformly; 3) transferring the mixed solution in the lining of the hydrothermal kettle in 2) into the hydrothermal kettle, heating it to 120-250° C., keeping the temperature constant for 1-50 hours, and then naturally cooling it to room temperature to obtain a nano sodium vanadium fluorophosphate powder; 4) heating the sodium vanadium fluorophosphate powder obtained in 3) to 400-800° C. at a heating rate of 1-10° C. / min under an inert atmosphere, keeping the temperature constant for 0.1-10 hours, and then naturally cooling it to room temperature to obtain a carbon-coated nano sodium vanadium fluorophosphate positive electrode material.
[0021] Advantages of the present invention:
[0022] The present invention adopts the strategy of simultaneously shortening the transmission distance of electrons and ions in the crystal during the charge and discharge process and simultaneously improving the electronic conductivity of the material surface, and prepares a nano sodium vanadium fluorophosphate / carbon composite material by a solvothermal method for synthesizing nanomaterials and combining a high-temperature annealing in-situ carbon coating method.
[0023] The nano sodium vanadium fluorophosphate / carbon composite material designed by the present invention has few defects, uniform particles, large specific surface area, short electron / ion transmission distance, excellent capacity rate performance, and ultra-long cycle life. The nano composite material obtained by controlling the particle size has a larger specific surface area and more reactive sites, a small volume change during charge and discharge, and will not break or fall off, which can effectively improve the rate and cycle performance of the material.
[0024] The carbon source of the present invention is used as a carbon coating material, and the carbon content in the reaction-generated material accounts for 0.1-10%. Through in-situ carbon coating, the electronic conductivity of the surface of the material particles can be greatly improved.
[0025] The preparation method of the nano sodium vanadium fluorophosphate / carbon composite material of the present invention has simple process and excellent performance, and is of great significance to the future application of long-life sodium ion batteries in the field of energy storage.
[0026] The nano sodium vanadium fluorophosphate / carbon composite material prepared by the present invention conforms to the tetragonal phase crystal structure and P42 / mnm point group structure of sodium vanadium fluorophosphate through X-ray diffraction testing, and the electrochemical performance test results show that the nanocomposites with different morphologies have excellent cycle stability and significantly enhanced capacity rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a microscopic SEM image of the sample of Example 1 of the present invention;
[0028] Figure 2 This is a microscopic SEM image of the sample of Example 2 of the present invention;
[0029] Figure 3 It is a microscopic SEM image of the comparative example sample of the present invention;
[0030] Figure 4 The XRD pattern of the sample of Example 1 of the present invention;
[0031] Figure 5 The electrochemical performance curves of Example 1 of the present invention and the comparative example samples are shown in FIG. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0033] A method for preparing a nano sodium vanadium fluorophosphate positive electrode material comprises the following steps:
[0034] 1) taking a sodium source, a vanadium source, a fluorine source and a phosphorus source respectively according to the element mass ratio Na:V:P:F=x:2:2:3, and taking a carbon source, wherein 3<x<6;
[0035] 2) adding the vanadium source, sodium source, fluorine source and carbon source in 1) into the inner lining of the hydrothermal kettle in sequence, and then adding the organic solvent and phosphorus source, stirring and mixing evenly;
[0036] 3) transferring the mixed solution in the lining of the hydrothermal kettle in 2) to the hydrothermal kettle, heating it to 120-250° C., keeping the temperature constant for 1-50 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder, namely Na3V2(PO4)2F3;
[0037] 4) The sodium vanadium fluorophosphate powder obtained in 3) is heated to 400-800° C. at a heating rate of 1-10° C. / min under an inert atmosphere, kept at a constant temperature for 0.1-10 h, and then naturally cooled to room temperature to obtain a carbon-coated nano sodium vanadium fluorophosphate positive electrode material.
[0038] 2) The medium carbon source is used as in-situ carbon coating to improve the electronic conductivity of the material surface.
[0039] The vanadium source in 1) is one or more of ammonium metavanadate, vanadium pentoxide, vanadium trichloride, vanadium tribromide, vanadium trioxide, vanadium acetylacetonate and vanadyl sulfate; the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and ammonium phosphate; the carbon source is formic acid (HCOOH), gallic acid (C7H6O5·H2O), oxalic acid (H2C2O4·2H2O), tartaric acid (C4H6O6), malic acid (C4H6O5), citric acid (C6H8O7·H2O) and EDTA (C 10 H 16 N2O8), wherein the carbon element in the carbon source is 150 to 300% of the molar number of the vanadium element.
[0040] The sodium source in 2) is one or more of sodium fluoride, sodium chloride, sodium carbonate, sodium hydroxide, sodium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium citrate, sodium oxalate, sodium phosphate and sodium nitrate; the fluoride source is one or more of sodium fluoride, ammonium fluoride, potassium fluoride and magnesium fluoride.
[0041] The organic solvent in 2) is one or more of methanol, ethanol, ethylene glycol, ethylenediamine, acetonitrile, acetone, nitromethane, dimethylformamide, triethylamine, dimethyl sulfoxide, butyrolactone and propylene carbonate, and the amount of the solvent is 60% of the volume of the hydrothermal autoclave.
[0042] In the step 2), the stirring speed is 100-800 r / min, the stirring temperature is 10-100° C., and the stirring time is 0.1-2 h.
[0043] The inert atmosphere in 4) is one or more of argon, argon-hydrogen mixed gas and nitrogen.
[0044] The invention also discloses a carbon-coated nano sodium vanadium fluorophosphate positive electrode material prepared by a method for preparing the nano sodium vanadium fluorophosphate positive electrode material.
[0045] The carbon-coated nano sodium vanadium fluorophosphate positive electrode material is a structure formed by agglomeration of amorphous carbon-coated nano-sheet sodium vanadium fluorophosphate primary particles.
[0046] The invention also discloses the application of a carbon-coated nano sodium vanadium fluorophosphate positive electrode material in a sodium ion battery.
[0047] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0048] Embodiment 1:
[0049] (1) Weigh 0.004 mol of ammonium metavanadate, 0.002 mol of citric acid, 0.006 mol of sodium fluoride, and 0.004 mol of diammonium phosphate;
[0050] (2) adding the ammonium metavanadate, citric acid, and sodium fluoride weighed in step (1) to the inner lining of a hot kettle containing water, and then adding methanol and ammonium dihydrogen phosphate, stirring for 0.5 hours in a water bath at 80° C. with a magnetic stirring rotor speed of 400 r / min until a light green precursor solution is formed;
[0051] (3) transferring the precursor solution in step (2) to a hydrothermal reactor, heating it to 180° C., keeping the temperature constant for 10 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder;
[0052] (4) The nano sodium vanadium fluorophosphate powder in step 3) is heated to 600° C. at a heating rate of 4° C. / min under an inert atmosphere, kept at the constant temperature for 0.5 h, and then naturally cooled to room temperature to obtain an amorphous carbon-coated nano sodium vanadium fluorophosphate (nano sodium vanadium fluorophosphate / carbon) composite positive electrode material.
[0053] Embodiment 2:
[0054] (1) Weigh 0.004 mol of vanadium trichloride, 0.001 mol of tartaric acid, 0.006 mol of ammonium fluoride, 0.003 mol of sodium carbonate and 0.004 mol of phosphoric acid;
[0055] (2) adding the vanadium trichloride, tartaric acid, ammonium fluoride and sodium carbonate weighed in step (1) to the inner lining of a hot kettle containing water, and then adding ethylenediamine and phosphoric acid, stirring for 1 hour in a water bath at 70° C. with a magnetic stirring rotor speed of 300 r / min until a light green precursor solution is formed;
[0056] (3) transferring the precursor solution in step (2) to a hydrothermal reactor, heating it to 200° C., keeping the temperature constant for 16 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder;
[0057] (4) The nano sodium vanadium fluorophosphate powder in step 3) is heated to 400° C. at a heating rate of 1° C. / min under an inert atmosphere, kept at the constant temperature for 10 h, and then naturally cooled to room temperature to obtain an amorphous carbon-coated nano sodium vanadium fluorophosphate (nano sodium vanadium fluorophosphate / carbon) composite positive electrode material.
[0058] Embodiment 3:
[0059] (1) Weigh 0.002 mol of vanadium pentoxide, 0.002 mol of malic acid, 0.002 mol of ammonium fluoride, and 0.004 mol of disodium hydrogen phosphate;
[0060] (2) adding the vanadium pentoxide, malic acid, and ammonium fluoride weighed in step (1) to the inner lining of a hot kettle containing water, and then adding triethylamine and disodium hydrogen phosphate, stirring for 0.1 hour in a water bath at 100° C. with a magnetic stirring rotor speed of 600 r / min until a light green precursor solution is formed;
[0061] (3) transferring the precursor solution in step (2) to a hydrothermal reactor, heating it to 250° C., keeping the temperature constant for 1 hour, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder;
[0062] (4) The nano sodium vanadium fluorophosphate powder in step 3) is heated to 800° C. at a heating rate of 10° C. / min under a nitrogen atmosphere, kept at this temperature for 0.1 h, and then naturally cooled to room temperature to obtain an amorphous carbon-coated vanadium-based fluorophosphate single crystal (vanadium-based fluorophosphate / carbon) positive electrode material.
[0063] Embodiment 4:
[0064] (1) Weigh 0.005 mol of vanadyl sulfate, 0.005 mol of oxalic acid dihydrate, 0.0075 mol of sodium fluoride, and 0.005 mol of potassium dihydrogen phosphate;
[0065] (2) adding the vanadyl sulfate, oxalic acid, and sodium fluoride weighed in step (1) to the inner lining of a hot kettle containing water, and then adding ethylene glycol and diammonium hydrogen phosphate, stirring for 2 hours in a water bath at 100° C. with a magnetic stirring rotor speed of 500 r / min until a light green precursor solution is formed;
[0066] (3) transferring the precursor solution in step (2) to a hydrothermal reactor, heating it to 120° C., keeping the temperature constant for 50 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder;
[0067] (4) The nano sodium vanadium fluorophosphate powder prepared in step 3) is heated to 600° C. at a heating rate of 1° C. / min in an argon-hydrogen mixed atmosphere, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain an amorphous carbon-coated vanadium-based fluorophosphate single crystal (vanadium-based fluorophosphate / carbon) positive electrode material.
[0068] Comparative Example:
[0069] Vanadium-based fluorophosphate polycrystalline (Na3V2O2(PO4)2F) material is prepared according to the sol-gel-high temperature sintering method, and the following steps are performed:
[0070] (1) Weigh 0.02 mol of ammonium metavanadate, 0.025 mol of oxalic acid dihydrate, 0.03 mol of sodium fluoride, and 0.02 mol of ammonium dihydrogen phosphate;
[0071] (2) dissolving the ammonium metavanadate and oxalic acid dihydrate weighed in step (1) into 100 ml of deionized water, stirring for 6 hours in a water bath at 80° C. with a magnetic stirring rotor speed of 500 r / min until a light green solution is formed, and then dissolving the weighed sodium fluoride and ammonium dihydrogen phosphate in the solution to form a precursor solution;
[0072] (3) the precursor solution obtained in step (2) is continuously stirred and heated to evaporate the solvent, and finally a sol-gel precursor 1 is obtained. The precursor 1 is dried by forced air at 80° C. for 12 h, and then ground for 20 min to obtain a uniform powder precursor 2;
[0073] (4) The powdered precursor 2 in step (3) was transferred to a tubular furnace and annealed under Ar atmosphere protection, heated to 600° C. at a heating rate of 4° C. / min, kept at a constant temperature for 8 h, and then naturally cooled to room temperature to obtain a control group sodium vanadium fluorophosphate / carbon positive electrode material.
[0074] A series of physical properties of the sodium vanadium fluorophosphate / carbon composite positive electrode material prepared in Example 1 were characterized. Figures 1 to 4 shown.
[0075] in, Figure 1 This is a SEM image of the nano sodium vanadium fluorophosphate / carbon composite material in Example 1, indicating that the prepared material has a relatively regular nanosheet structure.
[0076] Figure 2This is a SEM image of the nano sodium vanadium fluorophosphate / carbon composite material in Example 2, which shows that the material prepared by changing the raw materials is still a regular nanosheet structure, but the material size can be adjusted.
[0077] Figure 3 This is a SEM image of a comparative example sodium vanadium fluorophosphate polycrystalline material, illustrating that irregular polycrystalline particles are prepared by the sol-gel method.
[0078] Figure 4 This is an XRD comparison diagram of the sodium vanadium fluorophosphate / carbon composite material prepared in Example 1 and the comparative example. The X-ray diffraction test results show that the prepared nanomaterial has better crystallinity.
[0079] The sodium vanadium fluorophosphate / carbon composite material, conductive agent super P / carbon nanotube and binder CMC prepared in Example 1 and the comparative example were mixed in a ratio of 7:2:1 and dissolved in ultrapure water. The slurry was scraped onto aluminum foil and dried and rolled. The cut pieces were used as the positive electrode, the metal sodium sheet was used as the negative electrode, the glass fiber membrane was used as the diaphragm, the solute was 1M NaPF6, the solvent was a mixture of EC (ethylene carbonate), PC (propylene carbonate) and DEC (diethyl carbonate) solvents in a volume ratio of 1:1:1, the additive was 5% FEC as the electrolyte, and the aluminum foil was used as the current collector. The batteries were assembled into CR2025 / CR2016 button-type sodium ion batteries and the electrochemical performance was tested. The results are as follows: Figure 5 As shown, the samples of sodium vanadium fluorophosphate / carbon composite materials prepared by the sol-gel method are inferior to the nano sodium vanadium fluorophosphate / carbon composite materials of Example 1 at current densities of 0.2C and 1C. After nano-sizing and in-situ carbon coating, the specific capacity and cycle stability of the material are significantly improved. After 500 cycles, the capacity retention rate of the comparative example and Example 1 is 93.9%, which is much higher than 75.6% of the comparative example, indicating that the synthesized nano sodium vanadium fluorophosphate / carbon composite material effectively improves the electrochemical performance of the material.
[0080] In view of the shortcomings of sodium vanadium fluorophosphate and the current research status, the present invention adopts a strategy of simultaneously improving the electronic conductivity of the material and shortening the transmission distance of electrons / ions in the crystal, and prepares a high-performance sodium vanadium fluorophosphate / carbon composite material through solvent thermal and high-temperature annealing synthesis, in-situ carbon coating and particle lamellar nano-crystallization, which significantly improves the electrochemical performance of the material, and is of great significance for the future application of the material in commercial sodium ion batteries.
[0081] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a nano sodium vanadium fluorophosphate positive electrode material, characterized in that: The following steps are included: 1) taking a sodium source, a vanadium source, a fluorine source and a phosphorus source respectively according to the element molar ratio of Na:V:P:F=x:2:2:3, and taking a carbon source, wherein 3<x<6; 2) adding the vanadium source, sodium source, fluorine source and carbon source in 1) into the inner lining of the hydrothermal kettle in sequence, and then adding the organic solvent and phosphorus source, stirring and mixing evenly; 3) transferring the mixed solution in the lining of the hydrothermal kettle in 2) to the hydrothermal kettle, heating it to 120-250° C., keeping the temperature constant for 1-50 hours, and then naturally cooling it to room temperature to obtain nano sodium vanadium fluorophosphate powder; 4) The sodium vanadium fluorophosphate powder obtained in 3) is heated to 400-800° C. at a heating rate of 1-10° C. / min under an inert atmosphere, kept at a constant temperature for 0.1-10 h, and then naturally cooled to room temperature to obtain a carbon-coated nano sodium vanadium fluorophosphate positive electrode material.
2. A method for preparing a nano sodium vanadium fluorophosphate positive electrode material as claimed in claim 1, characterized in that: The vanadium source in 1) is one or more of ammonium metavanadate, vanadium pentoxide, vanadium trichloride, vanadium tribromide, vanadium trioxide, vanadium acetylacetonate and vanadyl sulfate; the phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and ammonium phosphate; the carbon source is one or more of formic acid, gallic acid, oxalic acid, tartaric acid, malic acid, citric acid and EDTA, and the amount of carbon element in the carbon source is 150-300% of the molar number of vanadium element.
3. A method for preparing a nano sodium vanadium fluorophosphate positive electrode material according to claim 1, characterized in that: The sodium source in 2) is one or more of sodium fluoride, sodium chloride, sodium carbonate, sodium hydroxide, sodium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium citrate, sodium oxalate, sodium phosphate and sodium nitrate; the fluoride source is one or more of sodium fluoride, ammonium fluoride, potassium fluoride and magnesium fluoride.
4. A carbon-coated nano sodium vanadium fluorophosphate positive electrode material and its application as claimed in claim 1, characterized in that: The organic solvent in 2) is one or more of methanol, ethanol, ethylene glycol, ethylenediamine, acetonitrile, acetone, nitromethane, dimethylformamide, triethylamine, dimethyl sulfoxide, butyrolactone and propylene carbonate.
5. A method for preparing a nano sodium vanadium fluorophosphate positive electrode material according to claim 1, characterized in that: In the step 2), the stirring speed is 100-800 r / min, the stirring temperature is 10-100° C., and the stirring time is 0.1-2 h.
6. A method for preparing a nano sodium vanadium fluorophosphate positive electrode material according to claim 1, characterized in that: The inert atmosphere in 4) is one or more of argon, argon-hydrogen mixed gas and nitrogen.
7. A carbon-coated nano sodium vanadium fluorophosphate positive electrode material prepared by the method for preparing a nano sodium vanadium fluorophosphate positive electrode material as claimed in any one of claims 1 to 6.
8. The carbon-coated nano sodium vanadium fluorophosphate positive electrode material prepared by the method for preparing a nano sodium vanadium fluorophosphate positive electrode material according to claim 7, characterized in that: The carbon-coated nano sodium vanadium fluorophosphate positive electrode material is a structure formed by agglomeration of amorphous carbon-coated nano-sheet sodium vanadium fluorophosphate primary particles.
9. Use of the carbon-coated nano sodium vanadium fluorophosphate positive electrode material as claimed in claim 7 in a sodium ion battery.
Citation Information
Patent Citations
Method for controllably preparing vanadium sodium fluorophosphate positive electrode material
CN108682855A
Preparation method of phosphorus-based sodium-ion battery positive electrode material with excellent electrochemical performance
CN118047364A
Vanadium sodium fluorophosphate positive electrode material and application thereof
CN118164465A
Vanadium sodium phosphate positive electrode material, sodium ion battery, preparation method therefor, and use thereof
US20210167387A1
Cited By
Preparation method and application of capsule-hole-rich nano spherical manganese-doped sodium vanadium fluorophosphate positive electrode material
CN121044563A
Positive electrode material and preparation method therefor, positive electrode sheet, and secondary battery
WO2026137505A1