Preparation method and application of wood-based nano material for electrolyzing urea in seawater
By synthesizing multi-element doped nickel-phosphorus alloy catalysts on the wood channel structure, B,P-NiCoFe@PW nanomaterials were prepared, which solved the problem of high-active electrocatalysts required for urea oxidation reaction in seawater, and achieved high efficiency and low cost The urea oxidation and hydrogen evolution reaction demonstrated excellent catalytic activity and stability.
Patent Information
- Application Number
- CN202411056537.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, urea oxidation reaction (UOR) in seawater requires highly active electrocatalysts, but precious metal catalysts are scarce and costly, which limits the efficiency and feasibility of seawater urea oxidation.
By activating wood and synthesizing multi-element doped nickel-phosphorus alloy catalysts on its pore structure, B,P-NiCoFe@PW nanomaterials were prepared using electroless plating technology, and catalytic activity was improved using its multi-active center and synergistic effect. A urea oxidation reaction is achieved in seawater.
Achieving a current density of 100mAcm-2 at lower voltages (1.34V) with almost no attenuation within 100 hours, showing high activity and stability, reducing energy consumption, and designed for hydrogen production and urea Excellent UOR catalysts for wastewater treatment offer prospects.
Smart Images

Figure CN118979274A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electro-oxidation, and in particular relates to a preparation method and application of a wood-based nano material for electrolyzing urea in seawater. Background Art
[0002] Hydrogen energy produced by electrocatalytic water splitting has the characteristics of high energy density and zero carbon emissions, which is crucial to achieving a hydrogen economy and global carbon neutrality. However, the oxygen evolution reaction (1.23V), as a half-reaction of water splitting, has slow kinetics and seriously reduces the efficiency of overall water splitting. In order to reduce energy consumption, it is very desirable to seek oxidation reactions with low thermodynamic potential to replace OER. Urea oxidation reaction (CO(NH2)2+6OH - +N2+5H2O+CO3 2- +6e - ) is considered as a viable alternative due to its relatively low oxidation potential (0.37 V) and the fact that it can be derived from urea-rich wastewater. Considering the low availability of pure water, the use of abundant seawater as electrolyte has attracted increasing attention. However, due to the low availability of 6e in UOR, the - Transfer, highly active electrocatalysts are required to accelerate the reaction kinetics of urea oxidation in seawater. Although noble metal catalysts (e.g., Pt, Rh) have been shown to have excellent catalytic activity for UOR, their scarcity and rising prices hinder further development of practical applications. Therefore, the development of efficient and low-cost UOR electrocatalysts is a key issue to achieve efficient H2 production and removal of urea-containing wastewater. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a preparation method and application of a wood-based nanomaterial for electrolysis of urea in seawater.
[0004] A method for preparing a wood-based nanomaterial for electrolyzing urea in seawater is specifically completed by the following steps:
[0005] 1. Immerse the wood in a reducing solution of NaBH4 for activation for a period of time to obtain activated wood;
[0006] 2. The activated wood is placed in a constant temperature heated plating solution I to react for a period of time, and then taken out and vacuum dried to obtain NiCoP@PW;
[0007] The preparation method of the plating solution I described in step 2 is: dissolving NiSO4·6H2O, Co(CH3COO)2·4H2O, Na3C6H5O7·2H2O, CH3COONH4, and NaH2PO2·H2O in deionized water, and then adjusting the pH value of the solution to 9.0-9.5 with 20%-25% ammonia water by mass to obtain plating solution I;
[0008] 3. Plating NiCoP@PW in plating solution II for a period of time, replacing plating solution II at regular intervals, taking it out after the reaction is completed, washing it, and then vacuum drying it to obtain a wood-based nanomaterial for electrolysis of urea in seawater;
[0009] The preparation method of the plating solution II described in step three is: dissolve (NH4)2Fe·(SO4)2·6H2O, (NH4)2S2O8 and dimethylamine borane in deionized water to obtain plating solution II.
[0010] Principles and advantages of the present invention:
[0011] 1. The present invention utilizes natural three-dimensional (3D) porous wood and synthesizes a multi-element doped nickel-phosphorus alloy on the wood pore structure by chemical plating technology; wherein the alloying-modified nickel-based catalyst, the doping of non-metallic heteroatoms and the synergistic effect between multiple metals significantly increase the catalytic sites and improve the catalytic activity; the multiphase electrocatalyst can promote the adsorption / desorption of reaction intermediates and achieve a synergistic effect through multiple active centers, thereby improving the bifunctional UOR and HER performance;
[0012] 2. The study found that the excellent activity and stability of the wood-based nanomaterial B, P-NiCoFe@PW for electrolysis of urea in seawater prepared by the present invention are attributed to the synergistic effect of multiple active centers and the charge redistribution caused by doping; these neatly arranged microchannels and hierarchical porous structures in the wood skeleton can not only improve the hydrophilicity and gas repellency of the entire electrode, which is beneficial to the penetration of electrolyte and the release of bubbles, but also shorten the transmission distance of ions and intermediates, and accelerate the kinetic process; the wood-based nanomaterial B, P-NiCoFe@PW for electrolysis of urea in seawater prepared by the present invention only requires a voltage of 1.34V to achieve 100mAcm -2 The current density of 100 mA cm-2 was achieved at an applied voltage of 1.67 V. -2 The current density;
[0013] Third, this invention promotes the understanding of regulating electronic structure through heteroatom doping strategy and provides a bright prospect for designing excellent UOR catalysts for hydrogen production and urea wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Schematic diagram of preparing wood skeleton-B, P-NiCoFe in Example 1;
[0015] Figure 2This is a scanning electron microscope image of the Paulownia wood in Example 1, with a magnification of 5000;
[0016] Figure 3 This is a scanning electron microscope image of the NiCoP@PW prepared in step 2 of Example 1, where (a) is at a magnification of 2000 and (b) is at a magnification of 20000;
[0017] Figure 4 This is a scanning electron microscope image of B,P-NiCoFe@PW prepared in step 3 of Example 1, with a magnification of 2000;
[0018] Figure 5 XRD patterns of NiCoP@PW and B,P-NiCoFe@PW prepared in Example 1;
[0019] Figure 6 A high-resolution transmission electron micrograph of B,P-NiCoFe@PW prepared in Example 1;
[0020] Figure 7 is the contact angle, where (a) is PW, (b) is NiCoP@PW, and (c) is B,P-NiCoFe@PW;
[0021] Figure 8 is the underwater bubble contact angle, where (a) is PW, (b) is NiCoP@PW, and (c) is B,P-NiCoFe@PW;
[0022] Fig. 9 OER and UOR performance of B,P-NiCoFe@PW prepared in Example 1 in 1M KOH and 1M KOH+0.33M urea;
[0023] Fig.10 Tafel of OER and UOR of B,P-NiCoFe@PW prepared in Example 1 in 1M KOH and 1M KOH+0.33M urea;
[0024] Fig.11 HER performance of B,P-NiCoFe@PW prepared in Example 1 in 1M KOH and 1M KOH+0.33M urea;
[0025] Fig.12 UOR performance of NiCoP@PW and B,P-NiCoFe@PW prepared in Example 1;
[0026] Fig.13 Polarization curves of HER||UOR and HER||OER of B,P-NiCoFe@PW prepared in Example 1 in different electrolytes;
[0027] Fig.14 It curve of HER||UOR assembled using B,P-NiCoFe@PW prepared in Example 1. DETAILED DESCRIPTION
[0028] Specific implementation method 1: This implementation method is a method for preparing a wood-based nanomaterial for electrolysis of urea in seawater, which is specifically completed according to the following steps:
[0029] 1. Immerse the wood in a reducing solution of NaBH4 for activation for a period of time to obtain activated wood;
[0030] 2. The activated wood is placed in a constant temperature heated plating solution I to react for a period of time, and then taken out and vacuum dried to obtain NiCoP@PW;
[0031] The preparation method of the plating solution I described in step 2 is: dissolving NiSO4·6H2O, Co(CH3COO)2·4H2O, Na3C6H5O7·2H2O, CH3COONH4, and NaH2PO2·H2O in deionized water, and then adjusting the pH value of the solution to 9.0-9.5 with 20%-25% ammonia water by mass to obtain plating solution I;
[0032] 3. Plating NiCoP@PW in plating solution II for a period of time, replacing plating solution II at regular intervals, taking it out after the reaction is completed, washing it, and then vacuum drying it to obtain a wood-based nanomaterial for electrolysis of urea in seawater;
[0033] The preparation method of the plating solution II described in step three is: dissolve (NH4)2Fe·(SO4)2·6H2O, (NH4)2S2O8 and dimethylamine borane in deionized water to obtain plating solution II.
[0034] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the preparation method of the NaBH4 reduction solution described in step 1 is: dissolving NaBH4 and NaOH in deionized water to obtain a NaBH4 reduction solution; the concentration of NaBH4 in the NaBH4 reduction solution is 3g / L to 8g / L, and the concentration of NaOH is 1g / L to 3g / L. The other steps are the same as those in specific embodiment 1.
[0035] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the wood material in step 1 is paulownia wood; the activation time in step 1 is 10 to 20 minutes. The other steps are the same as those in specific implementation method 1 or 2.
[0036] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the temperature of the plating solution I in step 2 is 50°C to 70°C; the reaction time in step 2 is 10min to 30min. The other steps are the same as those in specific embodiments 1 to 3.
[0037] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the vacuum drying temperature in step 2 is 50° C. to 70° C. and the vacuum drying time is 20 h to 28 h. The other steps are the same as those in specific embodiments 1 to 4.
[0038] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the concentration of NiSO4·6H2O in the plating solution I described in step 2 is 20g / L to 40g / L, the concentration of Co(CH3COO)2·4H2O is 0.5g / L to 1.5g / L, the concentration of Na3C6H5O7·2H2O is 20g / L to 40g / L, the concentration of CH3COONH4 is 10g / L to 15g / L, and the concentration of NaH2PO2·H2O is 20g / L to 30g / L. The other steps are the same as those of specific embodiments 1 to 5.
[0039] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the reaction temperature in step 3 is room temperature, the reaction time is 1h to 3h, and the plating solution II is replaced every 0.5h to 1h in step 3. The other steps are the same as those in specific embodiments 1 to 6.
[0040] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: the cleaning described in step 3 is performed using deionized water for 3 to 5 times; the vacuum drying temperature described in step 3 is 50°C to 70°C, and the vacuum drying time is 20h to 24h. The other steps are the same as those of specific embodiments 1 to 7.
[0041] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the concentration of (NH4)2Fe·(SO4)2·6H2O in the plating solution II described in step 3 is 4g / L to 6g / L, the concentration of (NH4)2S2O8 is 14g / L to 16g / L, and the concentration of dimethylamine borane is 2g / L to 4g / L. The other steps are the same as those of specific embodiments 1 to 8.
[0042] Specific embodiment ten: This embodiment is a wood-based nanomaterial for electrolysis of urea in seawater, which is used for urea electro-oxidation and hydrogen evolution reaction in alkaline seawater-urea electrolyte.
[0043] The following examples are used to verify the beneficial effects of the present invention:
[0044] Example 1: A method for preparing a wood-based nanomaterial (B, P-NiCoFe@PW) for electrolysis of urea in seawater, characterized in that the preparation method is specifically completed according to the following steps:
[0045] First, immersing paulownia wood (PW) in a reducing solution of NaBH4 for activation for 15 minutes to obtain activated wood;
[0046] The size of the paulownia wood described in step 1 is 1 cm×1.5 cm×0.2 cm;
[0047] The preparation method of the NaBH4 reducing solution described in step 1 is: dissolving NaBH4 and NaOH in deionized water to obtain a NaBH4 reducing solution; the concentration of NaBH4 in the NaBH4 reducing solution is 5 g / L, and the concentration of NaOH is 2 g / L;
[0048] 2. Place the activated wood in 100 mL of plating solution I at 60°C for 20 min, take it out and vacuum dry it at 60°C for 24 h to obtain NiCoP@PW;
[0049] The preparation method of the plating solution I described in step 2 is: dissolving NiSO4·6H2O, Co(CH3COO)2·4H2O, Na3C6H5O7·2H2O, CH3COONH4, and NaH2PO2·H2O into deionized water, and then adjusting the pH value of the solution to 9.5 with 25% ammonia water to obtain plating solution I;
[0050] The concentration of NiSO4·6H2O in the plating solution I described in step 2 is 30g / L, the concentration of Co(CH3COO)2·4H2O is 1g / L, the concentration of Na3C6H5O7·2H2O is 30g / L, the concentration of CH3COONH4 is 12g / L, and the concentration of NaH2PO2·H2O is 25g / L;
[0051] 3. NiCoP@PW was placed in 50 mL of plating solution II for reaction for 2 h, and the plating solution II was replaced every 1 h. After the reaction was completed, it was taken out, washed with deionized water for 3 times, and then vacuum dried at 60 ° C for 24 h to obtain a wood-based nanomaterial for electrolysis of urea in seawater (denoted as B,P-NiCoFe@PW);
[0052] The preparation method of the plating solution II described in step 3 is: dissolving (NH4)2Fe·(SO4)2·6H2O, (NH4)2S2O8 and dimethylamine borane (DMAB) in deionized water to obtain plating solution II;
[0053] The concentration of (NH4)2Fe·(SO4)2·6H2O in the plating solution II described in step three is 6 g / L, the concentration of (NH4)2S2O8 is 16 g / L, and the concentration of DMAB is 4 g / L.
[0054] Figure 2 This is a scanning electron microscope image of the Paulownia wood in Example 1, with a magnification of 5000;
[0055] Figure 3 This is a scanning electron microscope image of the NiCoP@PW prepared in step 2 of Example 1, where (a) is at a magnification of 2000 and (b) is at a magnification of 20000;
[0056] Figure 4 This is a scanning electron microscope image of B,P-NiCoFe@PW prepared in step 3 of Example 1, with a magnification of 2000;
[0057] By analyzing Figure 2 It was found that natural Paulownia wood showed an interconnected porous structure with a thinner cell wall layer, which shortened the transmission distance of electrolytes. Figure 3 The NiCoP alloy formed is uniformly deposited on the pore walls of the wood. By further introducing Fe and B nanoparticles on NiCoP@PW, the catalyst surface is made rougher, the specific surface area is increased, and the catalytic performance is enhanced. Figure 4 shown.
[0058] Figure 5 XRD patterns of NiCoP@PW and B,P-NiCoFe@PW prepared in Example 1;
[0059] Depend on Figure 5 It can be seen that NiCoP@PW and B,P-NiCoFe@PW both have Ni peaks (PDF#04-0850). Compared with the standard Ni peak, they all show a positive shift, indicating that the doping of heteroatoms leads to a decrease in the lattice constant of nickel. The decrease in the catalyst lattice constant will lead to an increase in lattice defects, grain refinement, and an increase in active sites, thereby improving the UOR activity.
[0060] Figure 6 A high-resolution transmission electron micrograph of B,P-NiCoFe@PW prepared in Example 1;
[0061] Figure 6 The lattice spacing of 0.20 nm is shown in FIG, corresponding to the (111) crystal plane of Ni.
[0062] The contact angles of PW, NiCoP@PW and B,P-NiCoFe@PW are shown in Figure 7 and Figure 8 As shown;
[0063] from Figure 7 It can be seen that compared with PW and NiCoP@PW, the water contact angle of B,P-NiCoFe@PW at 0.91s is only 11°. The results show that B,P-NiCoFe@PW has better hydrophilicity and can promote sufficient contact between active sites and reactive species. Figure 8 It shows that B,P-NiCoFe@PW also has good gas repellency, with an underwater bubble contact angle of 137°, which is higher than that of NiCoP@PW (125°) and PW (103°). This is crucial for the release of gas products produced on the catalyst surface at high current density. The hydrophilic and gas repellent surface structure helps to reduce the energy consumption of UOR / HER and improve the activity of the catalyst.
[0064] Urea electro-oxidation and hydrogen evolution performance:
[0065] The B, P-NiCoFe@PW prepared in Example 1 was immersed in a 1 mol / L KOH solution (1M KOH) and a 1M KOH+0.33M urea solution (a mixed solution of KOH and urea, with a KOH concentration of 1 mol / L and a urea concentration of 0.33 mol / L), respectively, to test the OER, UOR and HER performances of B, P-NiCoFe@PW. Figures 9-11 As shown;
[0066] Fig. 9 The OER and UOR performance of B,P-NiCoFe@PW prepared in Example 1;
[0067] Depend on Fig. 9 As shown in Figure 2, the UOR starting potential of B,P-NiCoFe@PW is 1.30 V, which is significantly lower than the OER starting potential (1.47 V). -2 At a current density of , the UOR overpotential is only 1.34V, while the OER overpotential requires 1.52V. This result proves that replacing OER with UOR can greatly reduce the overpotential and thus reduce energy consumption. In order to explore the reaction kinetics of the catalyst, Fig.10 The Tafel slopes based on the UOR and OER polarization curves are given. The Tafel slope of UOR is 49.0 mVdec -1 , lower than OER (62.5mVdec -1 ), indicating that UOR has better catalytic kinetic performance.
[0068] like Fig.11 As shown: The HER performance of B,P-NiCoFe@PW prepared in Example 1 in the two electrolytes is similar, indicating that urea has no significant effect on HER performance.
[0069] The UOR performance comparison of NiCoP@PW and B,P-NiCoFe@PW prepared in Example 1 is shown in Fig.12 ,from Fig.12 It can be seen that the performance of B,P-NiCoFe@PW is significantly better than that of NiCoP@PW, indicating that the dual doping of Fe and B significantly enhances the UOR activity.
[0070] The B,P-NiCoFe@PW prepared in Example 1 was used as cathode and anode, respectively, to assemble a full hydrolysis electrolyzer, and its HER||OER full hydrolysis activity was tested in 1 M KOH and 1 M KOH+seawater, and its HER||UOR full hydrolysis activity was tested in 1 M KOH+0.33 M urea and 1 M KOH+seawater+0.33 M urea.
[0071] Fig.13 1M KOH is a KOH solution with a concentration of 1 mol / L;
[0072] 1M KOH+0.33M urea is a mixed solution of KOH, urea and water, in which the concentration of KOH is 1 mol / L and the concentration of urea is 0.33 mol / L;
[0073] 1M KOH+seawater is a KOH seawater solution with a concentration of 1 mol / L;
[0074] 1M KOH+seawater+0.33M urea is a mixed solution of KOH, urea and seawater, in which the concentration of KOH is 1 mol / L and the concentration of urea is 0.33 mol / L;
[0075] like Fig.13 As shown: When reaching 100mAcm -2 At a current density of 1.64V, the voltage required in the 1M KOH+0.33M urea (1.64V) electrolyte and the 1M KOH+0.33M urea+seawater (1.67V) electrolyte is similar. Since seawater resources are relatively abundant and fresh water resources are scarce on the earth, it is of great significance to use seawater instead of fresh water as the electrolyte. Time (t)-current (i) is used to evaluate the cyclic stability of the material.
[0076] Depend on Fig.14 It can be seen that the B, P-NiCoFe@PW prepared in Example 1 are used as cathode and anode respectively, and the assembled HER||UOR reaches a current density of 100 mA cm -2 It can maintain stability for 200 hours.
Claims
1. A method for preparing a wood-based nanomaterial for electrolysis of urea in seawater, characterized in that The preparation method is specifically completed according to the following steps:
1. Immerse the wood in a reducing solution of NaBH4 for activation for a period of time to obtain activated wood; 2. The activated wood is placed in a constant temperature heated plating solution I to react for a period of time, and then taken out and vacuum dried to obtain NiCoP@PW; The preparation method of the plating solution I described in step 2 is: dissolving NiSO4·6H2O, Co(CH3COO)2·4H2O, Na3C6H5O7·2H2O, CH3COONH4, and NaH2PO2·H2O in deionized water, and then adjusting the pH value of the solution to 9.0-9.5 with 20%-25% ammonia water by mass to obtain plating solution I; 3. Plating NiCoP@PW in plating solution II for a period of time, replacing plating solution II at regular intervals, taking it out after the reaction is completed, washing it, and then vacuum drying it to obtain a wood-based nanomaterial for electrolysis of urea in seawater; The preparation method of the plating solution II described in step three is: dissolve (NH4)2Fe·(SO4)2·6H2O, (NH4)2S2O8 and dimethylamine borane in deionized water to obtain plating solution II.
2. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The preparation method of the NaBH4 reducing solution described in step 1 is: dissolving NaBH4 and NaOH in deionized water to obtain a NaBH4 reducing solution; the concentration of NaBH4 in the NaBH4 reducing solution is 3g / L~8g / L, and the concentration of NaOH is 1g / L~3g / L.
3. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The wood described in step one is paulownia wood; the activation time described in step one is 10 minutes to 20 minutes.
4. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The temperature of the plating solution I described in step 2 is 50° C. to 70° C.; the reaction time described in step 2 is 10 min to 30 min.
5. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The vacuum drying temperature in step 2 is 50° C. to 70° C., and the vacuum drying time is 20 h to 28 h.
6. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The concentration of NiSO4·6H2O in the plating solution I described in step 2 is 20g / L~40g / L, the concentration of Co(CH3COO)2·4H2O is 0.5g / L~1.5g / L, the concentration of Na3C6H5O7·2H2O is 20g / L~40g / L, the concentration of CH3COONH4 is 10g / L~15g / L, and the concentration of NaH2PO2·H2O is 20g / L~30g / L.
7. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The reaction temperature in step 3 is room temperature, and the reaction time is 1 h to 3 h; in step 3, the plating solution II is replaced every 0.5 h to 1 h.
8. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The cleaning described in step three is to use deionized water to clean for 3 to 5 times; the temperature of vacuum drying described in step three is 50° C. to 70° C., and the time of vacuum drying is 20 h to 24 h.
9. The method for preparing a wood-based nanomaterial for electrolysis of urea in seawater according to claim 1, characterized in that The concentration of (NH4)2Fe·(SO4)2·6H2O in the plating solution II described in step three is 4g / L~6g / L, the concentration of (NH4)2S2O8 is 14g / L~16g / L, and the concentration of dimethylamine borane is 2g / L~4g / L.
10. Use of a wood-based nanomaterial for electrolysis of urea in seawater prepared by the preparation method according to claim 1, characterized in that A wood-based nanomaterial for electrolysis of urea in seawater is used for urea electrooxidation and hydrogen evolution reaction in alkaline seawater-urea electrolyte.
Citation Information
Cited By
PAN modified NiCoP / NF catalyst for urea-assisted seawater electrolysis and preparation method of PAN modified NiCoP / NF catalyst
CN122082030A