Preparation method and application of phosphosilicic acid gel material

By using phosphosilicate gel material as an additive or alternative in proton exchange membrane fuel cells, the problems of high cost and complex processes in the prior art are solved, the proton conduction performance and peak power density of the fuel cells are improved, and fuel is promoted The commercial development of batteries.

CN118908217AInactive Publication Date: 2024-11-08BEIJING INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410951717.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The perfluorosulfonic acid resin materials used in existing proton exchange membrane fuel cells have high cost, complex synthesis processes and gas diffusion resistance problems, which limit the performance and commercial development of fuel cells.

Method used

Using phosphosilicate gel material as an additive or substitute, it is prepared through simple liquid phase reaction to optimize the molar ratio of silicon precursor to phosphorus precursor, and prepare gel materials with different phosphorus silicon ratios to improve proton exchange membrane fuel. Catalytic layer performance of the battery.

Benefits of technology

The proton conduction performance has been improved, the amount and cost of ionomers are reduced, the peak power density of fuel cells is increased, and the performance performance is improved by about 15%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908217A_ABST
    Figure CN118908217A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a phosphosilicic acid gel material, and belongs to the technical field of fuel cell materials. The phosphosilicic acid gel materials with different phosphorus-silicon ratios prepared by the method can be used as an additive to be compounded with # imgabs 0 #, or can be used as a substitute to replace part of # imgabs 1 # so as to realize the preparation of a novel ionomer composite material. The ionomer composite material can improve the performance of the fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cell materials, and in particular relates to a preparation method and application of a phosphosilicate gel material. Background Art

[0002] As an important component of proton exchange membrane fuel cells (PEMFC), ionomers play an important role in conducting protons in the fuel cell catalyst layer and ensuring efficient platinum catalysis. Currently, the most widely used ionomers are perfluorosulfonic acid resins produced by DuPont in the United States. The material itself has excellent proton conductivity and relatively good performance indicators. However, The close adsorption of the catalyst in the membrane electrode and the occupation of the active sites by the sulfonic acid groups lead to a higher gas diffusion resistance, which in turn affects the reaction inside the membrane electrode.

[0003] Although researchers have focused on existing commercial ionomers The optimization of The limitations of high cost and complicated synthesis process are still problems that need to be faced; at the same time, the slowdown and stagnation of new material development caused by technology monopoly will not be conducive to the further advancement of fuel cell research and development in the long run. In order to break the current situation of technology blockade, without sacrificing fuel cell performance, the development of Alternative materials or new composite materials to gradually reduce the system The usage is an important part of the commercial development of fuel cells.

[0004] The essence of new composite materials needs to meet the following three conditions: first, low cost and easy synthesis; second, The affinity is good and it is easy to realize compounding; thirdly, in terms of core properties, Remain consistent and have excellent proton conduction performance. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a preparation method and application of a phosphosilicate gel material.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] Technical solution 1:

[0008] A method for preparing a phosphosilicate gel material comprises the following steps: dissolving tetraethoxysilane in a hydrochloric acid aqueous solution to obtain a silicon precursor solution; adding phosphoric acid to the silicon precursor solution to obtain a phosphosilicate gel material; wherein the molar ratio of phosphorus in the phosphoric acid to silicon in the silicon precursor solution is 0.24-0.72, that is, the phosphorus-silicon ratio is 0.24-0.72.

[0009] Furthermore, the molar ratio of phosphorus in the phosphoric acid to silicon in the silicon precursor solution is 0.24, 0.48 or 0.72.

[0010] Furthermore, the hydrochloric acid aqueous solution is made of hydrochloric acid and water, and the usage ratio of tetraethoxysilane, hydrochloric acid and water is 5g:7.8μL:1.728g; the mass fraction of hydrochloric acid in the hydrochloric acid aqueous solution is 36%.

[0011] Technical solution 2:

[0012] The present invention also provides a phosphosilicate gel material prepared by the above preparation method.

[0013] Technical solution three:

[0014] An ionomer composite material, comprising a phosphosilicate gel material and a Composite; wherein the phosphosilicate gel material and The composite ratio (mass ratio) is (1-3): 1, preferably 1: 1 or 3: 1, more preferably 1: 1, or, the phosphosilicate gel material is used to replace part of the mass The substitution amount is 50 wt%.

[0015] Technical solution 4:

[0016] A method for preparing the ionomer composite material comprises the following steps: The phosphosilicate gel material is added into the mixture and stirred to obtain an ionomer composite material.

[0017] Technical solution five:

[0018] A use of the ionomer composite material in preparing electrode materials.

[0019] Technical solution six:

[0020] An application of the ionomer composite material in preparing a proton exchange membrane fuel cell.

[0021] Compared with the prior art, the present invention has the following advantages and technical effects:

[0022] 1) The present invention uses silicon precursors and phosphoric acid materials from a wide range of sources as raw materials, and prepares phosphosilicate gel through a simple liquid phase reaction. The impedance of the phosphosilicate gel at room temperature is 20 to 30 ohms, indicating that it has excellent proton conduction performance and can be used as additives or substitutes;

[0023] 2) The present invention prepares gel samples with different phosphorus-silicon ratios (measured phosphorus-silicon ratio is 0.12-0.39) by optimizing the ratio of silicon precursor to phosphorus precursor. The method is simple and easy to operate, avoiding cumbersome post-processing steps, and can be expanded to similar research systems;

[0024] 3) The phosphosilicate gel provided by the present invention can be used as an additive Compound, or as a substitute for part Then the preparation of new ionomer composite materials is realized. The introduction of gel can enhance the proton conduction in the catalyst layer. Therefore, the use of composite materials to prepare membrane electrodes can improve the performance of fuel cells. When phosphosilicate gel is used as an additive with Compared with the fuel cell without phosphosilicate gel, its peak power density can be increased by about 15%; when phosphosilicate gel replaces part of The obtained PEMFC peak power density is increased by up to about 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0026] Figure 1 The synthetic route of the phosphosilicate gel material of the present invention;

[0027] Figure 2 The XPS images and characteristic peak area integral values ​​of gel samples with different phosphorus-silicon ratios in Example 1 of the present invention, a is a phosphosilicate gel material with P / Si=0.24, b is a phosphosilicate gel material with P / Si=0.48, c is a phosphosilicate gel material with P / Si=0.72, and d is the actual phosphorus-silicon ratio of different phosphosilicate gel materials;

[0028] Figure 3 The polycrystalline powder X-ray diffractometer (PXRD) test results of the phosphosilicate gel material prepared in Example 1 are as follows: a is a phosphosilicate gel material with P / Si=0.24, b is a phosphosilicate gel material with P / Si=0.48, and c is a phosphosilicate gel material with P / Si=0.72;

[0029] Figure 4 Impedance spectra of the phosphosilicate gel material with P / Si=0.48 (actual phosphorus-silicon ratio is 0.31) and the phosphosilicate gel material with P / Si=0.72 (actual phosphorus-silicon ratio is 0.39) prepared in Example 1 at room temperature;

[0030] Figure 5The surface morphology of the membrane electrode prepared in Example 1 is characterized by SEM at a scale of 2 μm, wherein a, b, c, and d are the anode of the control group, the cathode of the control group, the cathode of the 1:1 group, and the cathode of the 3:1 group respectively;

[0031] Figure 6 This is the EDS and mapping characterization diagram of the membrane electrode cathode of the control group in Application Example 1;

[0032] Figure 7 The EDS and mapping characterization images of the 1:1 membrane electrode cathode in Application Example 1;

[0033] Figure 8 The effect of different proportions of phosphosilicate gel materials added under hydrogen-oxygen and hydrogen-air conditions on membrane electrode performance;

[0034] Fig. 9 The surface morphology of the membrane electrode prepared in Application Example 2 is characterized by SEM at a scale of 2 μm, wherein a, b, c, d, and e are the cathode of the control group, the cathode of the control group, the cathode with a phosphorus-silicon ratio of 0.24, the cathode with a phosphorus-silicon ratio of 0.48, and the cathode with a phosphorus-silicon ratio of 0.72, respectively;

[0035] Fig.10 This is the EDS and mapping characterization image of the membrane electrode cathode with a phosphorus-silicon ratio of 0.48 in Application Example 2;

[0036] Fig.11 This is the EDS and mapping characterization image of the membrane electrode cathode with a phosphorus-silicon ratio of 0.72 in Application Example 2;

[0037] Fig.12 The effect of different proportions of phosphosilicate gel materials added under hydrogen-oxygen and hydrogen-air conditions on membrane electrode performance;

[0038] Fig.13 The effect of partial replacement of commercial ionomers by phosphorus-silicon gel on membrane electrode performance under hydrogen-oxygen and hydrogen-air conditions. DETAILED DESCRIPTION

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0040] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0044] The present invention provides a preparation method and application of a cheap and readily available phosphosilicate gel material, which can be used as an additive or as a replacement for part of a perfluorosulfonic acid resin. A new type of ionomer composite material was prepared for use in the membrane electrode of proton exchange membrane fuel cells (PEMFC). The composite material can effectively improve the performance of fuel cells, and its peak power density is increased by about 15% compared with fuel cells without phosphosilicate gel. Phosphosilicate gel is easy to synthesize in batches and is expected to be used as Additives or substitutes can significantly reduce the cost of ionomers while ensuring or even improving the performance of PEMFC, which will be conducive to future commercial production.

[0045] The present invention can mix the silicon precursor and the phosphorus precursor materials in different proportions, and several proportions are preferably selected for experiments during the experiment. Different amounts of phosphosilicate gel can be added or different proportions of Only some proportions are preferred in the following examples. The acidic system involved in the present invention can be created not only by hydrochloric acid, but also by similar acids such as sulfuric acid and acetic acid. In addition, the reaction process involves reaction conditions not limited to standing at room temperature for 1 hour, and the temperature and standing time can be changed according to the specific situation.

[0046] The preparation method of the phosphosilicate gel material comprises the following steps:

[0047] 1) dissolving a silicon precursor (tetraethoxysilane, TEOS) in a hydrochloric acid aqueous solution and stirring thoroughly until TEOS is evenly dispersed in the water. This step is intended to obtain a silicon precursor solution in an acidic environment;

[0048] 2) adding different amounts of phosphoric acid to the solution to prepare solutions with different phosphorus-silicon ratios;

[0049] 3) Place the mixed solution at room temperature for a period of time to obtain gel samples with different phosphorus-silicon ratios (see the synthesis route for details). Figure 1 ).

[0050] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.

[0051] The raw materials used in the present invention are all purchased from the market.

[0052] The technical solution of the present invention is further illustrated by the following embodiments.

[0053] Example 1

[0054] Preparation of a phosphosilicate gel material:

[0055] 1) 5 g of TEOS, 1.728 g of ultrapure water, and 7.8 μL of 36% hydrochloric acid were mixed to obtain a mixed solution with obvious liquid stratification. A magnetic bar was added and the mixture was stirred on a magnetic stirrer for 35-40 min. After that, it was observed that the solution no longer stratified, and a completely dissolved TEOS aqueous solution was obtained;

[0056] 2) 0.4 mL, 0.8 mL and 1.2 mL of 85% by mass phosphoric acid were added dropwise to the TEOS aqueous solution, the bottle was capped, and the reaction was allowed to proceed at room temperature for 1 h to obtain phosphosilicate gel materials with P / Si=0.24, P / Si=0.48 and P / Si=0.72 (molar ratio, the same below), respectively.

[0057] Performance Testing:

[0058] 1. The phosphosilicate gel material prepared in Example 1 was subjected to an X-ray photoelectron spectroscopy (XPS) test. The results are as follows: Figure 2 shown. Figure 2 a in FIG. 1 is the XPS image of the phosphosilicate gel material with P / Si=0.24 in Example 1. Figure 2 b is the XPS image of the phosphosilicate gel material with P / Si=0.48 in Example 1, Figure 2 c in the figure is the XPS image of the phosphosilicate gel material with P / Si=0.72 in Example 1. Figure 2 d in the figure is the actual phosphorus-silicon ratio of different phosphosilicate gel materials in Example 1. The results show that the prepared samples contain phosphorus and silicon elements, and there are significant differences in the actual measured phosphorus-silicon ratios of samples with different feed ratios, which proves the successful preparation of phosphosilicate gel and confirms that there are indeed significant differences in the actual phosphorus-silicon ratios of the products obtained after adding reactants according to different feed ratios.

[0059] 2. The phosphosilicate gel material prepared in Example 1 was tested by a polycrystalline powder X-ray diffractometer (PXRD). The results are as follows: Figure 3 shown. Figure 3 a in FIG. 1 is the XRD image of the phosphosilicate gel material with P / Si=0.24 in Example 1. Figure 3 b is the XRD image of the phosphosilicate gel material with P / Si=0.48 in Example 1, Figure 3 c in FIG. 1 is the XRD pattern of the phosphosilicate gel material with P / Si=0.72 in Example 1. Figure 3 It can be seen that characteristic peaks appear in all three groups of gel samples, which further proves the successful preparation of phosphosilicate gel.

[0060] 3. Conductivity tests were performed on the phosphosilicate gel material with P / Si=0.48 (actual phosphorus-silicon ratio of 0.31) and the phosphosilicate gel material with P / Si=0.72 (actual phosphorus-silicon ratio of 0.39) prepared in Example 1. The results are as follows: Figure 4 As shown, the results show that the resistance of the two groups of phosphosilicate gels at room temperature is only twenty to thirty ohms, and the conductive properties are good.

[0061] Application Example 1

[0062] The phosphosilicate gel material with P / Si=0.24 in Example 1 is added as an additive to Ionomer composites were prepared by mixing phosphosilicate gel with The mixture was mixed in a mass ratio of 1:1 and 3:1. The specific preparation method was as follows: 17.28 mg of 17.28 mg and 51.84 mg of phosphosilicate gel were added into the system to prepare the ionomer composite material. The preparation process of membrane electrode mainly includes three parts: pulping, spraying and hot pressing. The specific method is: 1) Use an electronic balance to weigh 13.2 mg and 7.2 mg of commercial platinum-carbon catalyst in a glass bottle corresponding to the anode and cathode respectively; first add 0.1 mL of ultrapure water to each bottle to avoid the danger of sparks caused by the direct addition of organic solvents, and then use a pipette to measure 2.9 mL and 0.9 mL of isopropanol respectively and slowly add them to the bottle, cover the bottle cap, and place it in a nano-ultrasonic dispersion instrument with a controllable temperature not higher than 20°C for pre-dispersion for 1 hour. During the process, 31.68 mg of commercial ionomer perfluorosulfonic acid resin (20% ), disperse it in 1.4mL of isopropanol as the anode ionomer, and disperse the ionomer composite material in 1.4mL of isopropanol as the cathode ionomer, and pre-disperse them by ultrasonic treatment for 1h. After the material in the centrifuge tube is completely dispersed without obvious precipitation, use a dropper to suck out all the liquid in the centrifuge tube, and then add it dropwise to the glass bottle of the corresponding electrode, and ultrasonicate for 3h until there is no obvious particle deposition in the bottle, and the pulping is completed; 2) Use a nano-spraying device to spray the slurry on both sides of the proton exchange membrane; 3) Place the membrane electrode between two plastic gaskets with a 30mm×30mm hole cut out in the middle, and then use carbon paper to clamp the hole in the plastic gasket, sandwich it in aluminum foil, put it in a hot press at a pressure of 0.5MPa at 120℃ for 4min, take it out after the hot pressing is completed, and tear off the aluminum foil to obtain the required membrane electrode. Different membrane electrodes are obtained. With pure phosphosilicic acid gel material without adding The membrane electrode prepared by the sample was the control group.

[0063] Performance Test:

[0064] 1. The surface morphology of the prepared membrane electrode was characterized by scanning electron microscopy (SEM). Figure 5 shown. Figure 5 a in the figure is the anode of the control group. Figure 5 b is the cathode of the control group, Figure 5 The c in the figure is phosphosilicate gel and The mass ratio is 1:1 for a group of cathodes. Figure 5 The d in the equation is phosphosilicate gel and The mass ratio of the cathode group is 3:1. Figure 5 It shows that the slurry is evenly sprayed on the surface of the proton exchange membrane.

[0065] 2. Using the EDS and elemental surface analysis function (mapping) attached to the SEM, elemental analysis and tracing were performed on the surface of the control group membrane electrode cathode and the 1:1 group membrane electrode cathode. The results are as follows: Figure 6 , Figure 7 As shown. Figure 6 , Figure 7 It can be seen that the gel is uniformly dispersed in the ionomer system.

[0066] 3. The membrane electrode prepared in Example 1 was tested for polarization curve and power density curve in H2-Air fuel cell. The test conditions were: cathode loading was 0.05 mg Pt cm -2 , anode loading 0.1 mg Pt cm -2 , 80℃, 250kPaabs, the results are as follows Figure 8 As shown in a in .

[0067] The membrane electrode prepared in Example 1 was subjected to polarization curve and power density curve tests in a H2-O2 fuel cell. The test conditions were: the cathode loading was 0.05 mg Pt cm -2 , anode loading 0.1 mg Pt cm -2 , 80℃, 150kPaabs, the results are as follows Figure 8 As shown in b.

[0068] Figure 8 a in the figure shows that under hydrogen-air conditions, adding phosphosilicate at a ratio of 1:1 significantly improves the system performance (compared with the control group, the same below), and the power density is increased by about 4%. Figure 8 The figure b shows that the optimization effect brought by adding the same proportion of hydrogen and oxygen under the condition of water is relatively large, and the power density is increased by about 10%. In summary, under the condition of appropriate addition ratio, the performance optimization effect of phosphosilicate gel on the membrane electrode system is optimal.

[0069] Application Example 2

[0070] The phosphosilicate gel materials with P / Si=0.24, P / Si=0.48 and P / Si=0.72 in Example 1 were added as additives. Preparation of ionomer composites, phosphosilicate gel and The mass ratio of phosphosilicate gel material was 1:1, and three groups of membrane electrodes were prepared. The preparation method was the same as that in Application Example 1. The membrane electrode prepared by the sample was the control group.

[0071] Performance Testing:

[0072] 1. The surface morphology of the prepared membrane electrode was characterized by scanning electron microscopy (SEM). Fig. 9 shown. Fig. 9 a in the figure is the anode of the control group without adding gel sample. Fig. 9 b in the figure is the cathode of the control group without adding gel sample. Fig. 9 The c in the figure is a cathode with a phosphorus-silicon ratio of 0.24. Fig. 9 The d in the figure is a cathode with a phosphorus-silicon ratio of 0.48. Fig. 9 The e in the figure is a cathode with a phosphorus-silicon ratio of 0.72. Fig. 9 The results showed that the slurry was well dispersed on the membrane surface without agglomeration.

[0073] 2. Use the EDS and elemental surface analysis function (mapping) of the SEM to perform elemental analysis and tracing on the surface of each group of membrane electrodes. The results are as follows: Figure 7 , 10 -11. Figure 7This is the EDS and mapping characterization diagram of the membrane electrode cathode with a phosphorus-silicon ratio of 0.24. Fig.10 This is the EDS and mapping characterization diagram of the membrane electrode cathode with a phosphorus-silicon ratio of 0.48. Fig.11 This is the EDS and mapping characterization diagram of the membrane electrode cathode with a phosphorus-silicon ratio of 0.72. Figure 7 , 10 -11 It can be seen that the gel is evenly dispersed in the ionomer system, and the battery slurry also exists on the membrane surface and is evenly distributed.

[0074] 3. The prepared membrane electrode was tested for polarization curve and power density curve in H2-O2 fuel cell. The test conditions were: cathode loading was 0.05 mgPtcm -2 , anode loading 0.1mgPtcm -2 , 80℃, 150kPaabs, the results are as follows Fig.12 As shown in a in .

[0075] The prepared membrane electrode was tested for polarization curve and power density curve in H2-Air fuel cell. The test conditions were: cathode loading was 0.05 mgPtcm -2 , anode loading 0.1mgPtcm -2 , 80℃, 250kpa abs , the results are as follows Fig.12 As shown in b.

[0076] Fig.12 It shows that under hydrogen and oxygen conditions, the system with a phosphorus-silicon ratio of 0.48 (actually measured to be 0.31) has better performance, with a peak power density increased by 11% compared with the control group. The results under hydrogen and air conditions are basically the same. The system with a phosphorus-silicon ratio of 0.48 is still the best performing group, with a peak power density increased by 8.4% compared with the control group.

[0077] Application Example 3

[0078] The phosphosilicate gel material with P / Si=0.48 in Example 1 was used to replace 50wt% of the That is, the total mass of the raw materials remains unchanged, and the silica gel material and The mass ratio of Nafion to silica gel material is 1:1, and a membrane electrode is prepared. The preparation method is the same as that of Application Example 1 (replacement means that the total mass of the raw materials remains unchanged. The original raw material is only Nafion, and now half of the mass of Nafion is replaced by silica gel material; when added in the form of an additive, it means that the total mass of the raw materials will change. The original raw material is only Nafion, and now additional silica gel material is added, and the mass ratio of the two is 1:1).

[0079] Performance Testing:

[0080] The prepared membrane electrode was heated to 400 °C in H 2- Polarization curve and power density curve test in O2 fuel cell, the test conditions are: cathode loading is 0.05mg Pt cm -2 , anode loading 0.1 mg Pt cm -2 , 80℃, 150kpa abs , the results are as follows Fig.13 As shown in a in .

[0081] The prepared membrane electrode was exposed to H 2- Polarization curve and power density curve test were carried out in Air fuel cell. The test conditions were: cathode loading was 0.05 mg Pt cm -2 , anode loading 0.1 mg Pt cm -2 , 80℃, 250kpa abs , the results are as follows Fig.13 As shown in b.

[0082] Fig.13 It shows that the use of phosphosilicate gel can partially replace the It not only reduces fuel cell costs, but also improves performance.

[0083] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a phosphosilicate gel material, characterized in that: The following steps are involved: dissolving tetraethoxysilane in aqueous hydrochloric acid to obtain a silicon precursor solution; Phosphoric acid is added to the silicon precursor solution to obtain a phosphosilicate gel material; wherein the molar ratio of phosphorus in the phosphoric acid to silicon in the silicon precursor solution is 0.24-0.

72.

2. The method for preparing the phosphosilicate gel material according to claim 1, characterized in that: The molar ratio of phosphorus in the phosphoric acid to silicon in the silicon precursor solution is 0.24, 0.48 or 0.

72.

3. The method for preparing the phosphosilicate gel material according to claim 1, characterized in that: The hydrochloric acid aqueous solution is made of hydrochloric acid with a mass fraction of 36% and water, and the usage ratio of tetraethoxysilane, hydrochloric acid and water is 5g:7.8μL:1.728g.

4. A phosphosilicate gel material prepared by the preparation method according to any one of claims 1 to 3.

5. An ionomer composite material, characterized in that: The phosphosilicate gel material according to claim 4 is used as an additive and Composite; wherein the phosphosilicate gel material and The composite ratio is (1-3):

1.

6. An ionomer composite material, characterized in that: The phosphosilicate gel material according to claim 4 is used to replace part of the mass The substitution amount is 50 wt%.

7. A method for preparing an ionomer composite material according to claim 5 or 6, characterized in that: The following steps are included: The phosphosilicate gel material is added into the mixture and stirred to obtain an ionomer composite material.

8. Use of the ionomer composite material according to claim 5 or 6 in preparing electrode materials.

9. Use of the ionomer composite material according to claim 5 or 6 in the preparation of a proton exchange membrane fuel cell.

Citation Information

Patent Citations

  • Free-standing composite proton conducting film and preparation method thereof

    CN101789278A

  • Fuel cell catalyst layer and fuel cell

    CN114361469A

  • Production of catalyst-coated polymer electrolyte membrane, used in electrochemical cell, e.g. fuel cell, uses temperature near glass transition temperature of ionomer in tempering membrane coated with catalyst formulation

    DE102004059695A1

  • Fuel cell system for vehicle, has flow channels for flowing humidifying mediums that are formed in separator plates at different locations, and moistening device that is set to moisten electrolyte membrane with humidifying mediums

    DE102012011863A1

  • Phosphosilicate gel, proton conductive material and its production method

    JP2003137527A