A Green Synthesis Method for MWW-Structured Molecular Sieves
By using Y molecular sieves and MCM-22 seed crystals to synthesize MWW-structured molecular sieves under dynamic hydrothermal conditions, the problems of high cost and environmental hazards have been solved, realizing low-cost and environmentally friendly molecular sieve synthesis, which is suitable for catalytic cracking and aromatization reactions.
Patent Information
- Application Number
- CN202411009338.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The synthesis of existing MWW-structured molecular sieves is costly and uses the highly toxic template agent cycloheximine, which leads to environmental and health hazards. In addition, the traditional synthesis cycle is long, making it difficult to achieve green and efficient industrial applications.
Using Y-type molecular sieves with a suitable silicon-to-aluminum ratio as the parent material and combined with MCM-22 molecular sieve seed crystals, MWW-structured molecular sieves were synthesized under dynamic hydrothermal conditions, avoiding the use of cycloheximine template agents. By controlling crystallization conditions such as temperature, time, and stirring rate, the crystallization cycle was shortened.
The low-cost, environmentally friendly synthesis of MWW-structured molecular sieves has been achieved, with a shortened crystallization cycle, and it has good prospects for industrial application.
Smart Images

Figure CN118908241B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials synthesis, and in particular relates to a green synthesis method for MWW molecular sieves. Background Technology
[0002] MWW-structured molecular sieves, typified by MCM-22, are a novel molecular sieve configuration first developed and synthesized by Mobil in 1990 (US 4954325, 1990). These sieves possess two independent pore systems: a ten-membered ring sinusoidal cross-channel system and a twelve-membered ring supercage system. They exhibit excellent catalytic performance in reactions such as catalytic cracking, alkylation, and aromatization, attracting widespread attention from researchers in related fields. However, the conventional synthesis of MCM-22 uses expensive cycloheximine as a template agent (Zeolites, 1995, 15, 2; Micropor. Mesopor. Mater.; 1999, 31, 241.), resulting in high synthesis costs. Furthermore, its highly toxic properties pose significant risks to the environment and human health, and its transportation and use are subject to strict controls, severely restricting the production and industrial application of MWW-structured molecular sieves. Therefore, developing green synthetic methods for MWW-structured molecular sieves and reducing or avoiding the use of highly toxic cycloheximine template agents has become a goal pursued by researchers in this field. In the literature Chem. Asian J., 2017, 12, 530, a pre-made MCM-22 molecular sieve was used as a seed crystal to synthesize MWW-structured molecular sieves without the use of cycloheximine template agent, but the crystallization time required was 90-168 h.
[0003] The transcrystalline transformation phenomenon of molecular sieves is caused by the difference in thermodynamic stability among different types of molecular sieves and often occurs during traditional hydrothermal synthesis. Utilizing this phenomenon to synthesize certain molecular sieves with specific structures offers advantages over traditional hydrothermal synthesis, such as shorter crystallization cycles and avoidance of template agents (Chin. J. Catal., 2019, 40, 1854; J. Am. Chem. Soc. 2014, 136, 15280; Chem. Mater. 2023, 35, 4717.). The literature Chem. Mater. 2015, 27, 2056 systematically studied the transcrystalline transformation technology of molecular sieves, finding that when the parent molecular sieve and the target molecular sieve contain the same structural units, the target product can be synthesized through transcrystalline transformation without the use of template agents or seed crystals. FAU-structured molecular sieves (X, Y) can be synthesized without organic template agents and have low thermodynamic stability, often used as a parent material to prepare other types of molecular sieves through transcrystalline transformation. The literature *Micropor. Mesopor. Mater.*; 2014, 200, 269; *Micropor. Mesopor. Mater.*; 2016, 236, 54. and patent CN201410041274.5 synthesize MCM-49 molecular sieves with MWW structures using alumina-rich FAU molecular sieves (SiO2 / Al2O3 < 5.0). However, the synthesis process requires the addition of a large amount of silicon source, the parent molecular sieve accounts for less than 25% of the raw materials, and the crystallization process still requires a large amount of cycloheximine as a template agent. Therefore, developing a green synthesis method for MWW-structured molecular sieves with short crystallization cycles and low amounts of highly toxic template agents remains a goal that researchers are committed to achieving. Summary of the Invention
[0004] The present invention aims to overcome the shortcomings of the prior art and provide a green synthesis method for MWW structured molecular sieves that has a shortened crystallization cycle, low synthesis cost, and is environmentally friendly.
[0005] To solve the above-mentioned technical problems, the present invention is implemented as follows: A green synthesis method for MWW-structured molecular sieves involves uniformly mixing Y molecular sieves with an aluminum source, an alkali source, seed crystals, and deionized water, and then crystallizing the mixture under dynamic hydrothermal conditions to obtain the MWW-structured molecular sieve.
[0006] Furthermore, the SiO2 / Al2O3 molar ratio of the Y molecular sieve is 40 to 120.
[0007] Furthermore, the aluminum source is one or a mixture of two or more of sodium aluminate, aluminum nitrate, or aluminum sulfate.
[0008] Furthermore, the alkali source is one or a mixture of two of sodium hydroxide or potassium hydroxide.
[0009] Furthermore, the seed crystal is MCM-22 molecular sieve, and its mass ratio to Y molecular sieve is 0.1 to 0.4.
[0010] Furthermore, the crystallization conditions are: a stirring rate of 10–90 rpm, a temperature of 130–150°C, and a time of 36–84 h.
[0011] Furthermore, the molar composition of the synthesized system is SiO2: 0.03Al2O3: 0.16~0.19Na2O: 35~50H2O.
[0012] Compared with the prior art, the beneficial effects of this invention are that it uses Y molecular sieve with a suitable silicon-to-aluminum ratio as the parent material and uses pre-made MWW molecular sieve seed crystals to replace the highly toxic template agent cycloheximine to synthesize MWW molecular sieves. This shortens the crystallization cycle, reduces the synthesis cost, and is environmentally friendly. It has strong practicality, environmental protection and good prospects for industrial application. Attached Figure Description
[0013] Figure 1 This is the XRD pattern of the seed crystals used in this invention.
[0014] Figure 2 The image shows the XRD pattern of the sample obtained in Example 1 of this invention.
[0015] Figure 3 This is a SEM image of the sample obtained in Example 1 of the present invention.
[0016] Figure 4 This is an HRTEM image of the sample obtained in Example 1 of the present invention.
[0017] Figure 5 This is the physical adsorption isotherm diagram of the sample obtained in Example 1 of the present invention. Detailed Implementation
[0018] To enable those skilled in the art to better understand the technical solutions of this invention, the invention will be further described below with reference to specific embodiments. Obviously, the described embodiments are merely a part of the embodiments of this invention, and not all of them. These embodiments should be understood as being used only to illustrate the invention and not to limit the scope of protection of the invention. After reading the contents of this invention, all other embodiments obtained by making various modifications or alterations to the invention based on the technical solutions and embodiments of this invention also fall within the scope of protection of the claims of this invention.
[0019] The seed crystals (MCM-22) used in the experiment were prepared according to the reference (Micropor. Mesopor. Mater.; 1999, 31, 241.), with a SiO2 / Al2O3 molar ratio of 30, and were not subjected to calcination to remove the template agent. All other basic raw materials used were commercially available and used directly without special treatment.
[0020] Example 1 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.45 g of NaOH in 22.7 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel with a polytetrafluoroethylene liner and crystallize at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0021] Example 2 Synthesis of Molecular Sieves 0.101 g of sodium aluminate and 0.45 g of NaOH were dissolved in 22.7 mL of deionized water and stirred thoroughly. Then, 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 120) were added. The mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallized at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirmed that the synthesized sample was MCM-22.
[0022] Example 3 Synthesis of Molecular Sieves 0.03 g of sodium aluminate and 0.41 g of NaOH were dissolved in 19.6 mL of deionized water and stirred thoroughly. Then, 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40) were added. The mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel with a polytetrafluoroethylene liner and crystallized at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirmed that the synthesized sample was MCM-22.
[0023] Example 4 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.47 g of NaOH in 28.0 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel with a polytetrafluoroethylene liner and crystallize at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0024] Example 5 Synthesis of Molecular Sieves 0.03 g of sodium aluminate and 0.38 g of NaOH were dissolved in 19.2 mL of deionized water and stirred thoroughly. Then, 0.15 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40) were added. The mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallized at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirmed that the synthesized sample was MCM-22.
[0025] Example 6 Synthesis of Molecular Sieves 0.03 g of sodium aluminate and 0.484 g of NaOH were dissolved in 24.4 mL of deionized water and stirred thoroughly. Then, 0.60 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40) were added. The mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallized at 140 °C for 72 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirmed that the synthesized sample was MCM-22.
[0026] Example 7 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.45 g of NaOH in 22.7 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallize at 130 °C for 84 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0027] Example 8 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.45 g of NaOH in 22.7 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallize at 150 °C for 36 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0028] Example 9 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.45 g of NaOH in 22.7 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallize at 150 °C for 36 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0029] Example 10 Synthesis of Molecular Sieves 0.122 g of aluminum sulfate octahydrate and 0.45 g of NaOH were dissolved in 22.7 mL of deionized water and stirred thoroughly. Then, 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40) were added. The mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel with a polytetrafluoroethylene liner and crystallized at 150 °C for 36 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirmed that the synthesized sample was MCM-22.
[0030] Example 11 Synthesis of Molecular Sieves Dissolve 0.03 g of sodium aluminate and 0.63 g of KOH in 22.7 mL of deionized water. After thorough mixing, add 0.45 g of MCM-22 seed crystals and 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40). Stir continuously at room temperature for 0.5 h. Transfer the mixture to a stainless steel crystallization vessel with a polytetrafluoroethylene liner and crystallize at 150 °C for 36 h at a speed of 60 rpm. After centrifugation and washing, the solid product is dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis confirms that the synthesized sample is MCM-22.
[0031] Comparative Example 1: Synthesis of Molecular Sieves 0.03 g of NaAlO2 and 0.45 g of NaOH were dissolved in 22.7 mL of deionized water and stirred thoroughly. Then, 1.5 g of Y-molecular sieve (SiO2 / Al2O3 molar ratio 40) was added, and the mixture was stirred continuously at room temperature for 0.5 h. The mixture was then transferred to a stainless steel crystallization vessel lined with polytetrafluoroethylene and crystallized at 150 °C for 36 h at a speed of 60 rpm. After centrifugation and washing, the solid product was dried at 100 °C and calcined at 550 °C for 4 h in air. XRD analysis showed that the synthesized sample was a mixed crystal of ZSM-5 and mordenite.
[0032] It is understood that those skilled in the art can make various other corresponding changes and extensions based on the technical method of the present invention, and all such changes and extensions should fall within the protection scope of the claims of the present invention.
Claims
1. A green synthesis method of a MWW structure molecular sieve, characterized by: Mixing Y zeolite with aluminum source, alkali source, seed crystal and deionized water uniformly, crystallizing under dynamic hydrothermal condition, MWW structure molecular sieve is obtained; no silicon source and template are added in the synthesis system; the SiO2 / Al2O3 molar ratio of the Y zeolite is 40-120; the seed crystal is MCM-22 molecular sieve, and the mass ratio of the MCM-22 molecular sieve to the Y zeolite is 0.1-0.
4.
2. A green synthesis process of MWW structure molecular sieves according to claim 1, characterized by: The crystallization condition is that the stirring rate is 10-90 rpm, the temperature is 130-150 DEG C, and the time is 36-84 h.
3. The method of claim 2, wherein: The molar composition of the synthesis system is SiO2:0.03Al2O3:0.16-0.19Na2O:35-50H2O.
Citation Information
Patent Citations
A kind of method for preparing molecular sieve of MWW structure
CN104803396B
Method for preparing MWW structure molecular sieve
CN104803396A
Ultrasonic-assisted amine-free synthetic method for MWW molecular sieve
CN108423689A