Manganese dioxide electrode material, positive plate and preparation method thereof
Through ball milling method and aluminum ion doping technology, stable aluminum-doped manganese dioxide electrode materials were prepared, which solved the structural collapse and dissolution of manganese dioxide during charging and discharging, and improved the cycle stability of water-based secondary batteries. and active load, suitable for the positive electrode of aqueous zinc ion batteries.
Patent Information
- Application Number
- CN202410975939.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing manganese dioxide positive electrode materials are prone to structural collapse and dissolution during charging and discharging, resulting in poor cycle stability and rate performance, limiting the actual promotion and application of manganese-based water-based secondary batteries.
The defect-rich α-MnO2 was prepared by ball milling method of potassium permanganate and divalent manganese salts, and then in-situ aluminum doping was achieved through aluminum ion doping and water washing, and a solid-phase α-type dioxide was prepared by aluminum doping. Manganese electrode material improves the stability and activity of the material through low-temperature heat treatment and solution exchange technology.
It effectively inhibits the dissolution of manganese dioxide positive electrode, improves the circulation stability and active component load of water-based secondary batteries, and is suitable for the positive electrode of water-based zinc ion batteries, significantly improving the circulation performance of the material.
Smart Images

Figure CN118908282A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical energy storage, and in particular to a manganese dioxide electrode material, a positive electrode sheet and a preparation method thereof. Background Art
[0002] With the rapid development of new energy fields such as solar energy and wind energy, as well as the huge demand for peak shaving and valley filling in power grids, the requirements for the performance, cost and safety of large-scale energy storage devices are becoming increasingly higher. Aqueous secondary batteries are a new type of highly efficient and intrinsically safe rechargeable battery. They not only have the advantages of simple preparation process, non-toxic, low-cost, abundant sources of battery materials, and safe discharge process, but also have high energy density. Aqueous secondary batteries mainly include positive electrode materials, negative electrode materials, diaphragms, electrolytes, binders, current collectors and sealing materials. The positive electrode materials that can be used for aqueous secondary batteries reported in the prior art mainly include manganese-based, vanadium-based oxides and organic polymers, among which manganese dioxide has the characteristics of high capacity and low price, but it is easy to collapse and dissolve in the structure during the charge and discharge process, resulting in poor cycle stability and rate performance, which limits the actual promotion and application of manganese-based aqueous secondary batteries.
[0003] It should be noted that the information disclosed in the above background technology section is only used for understanding the background of the present application, and therefore may include information that does not constitute prior art known to ordinary technicians in the field. Summary of the invention
[0004] In order to make up for the deficiencies of the prior art, the present invention provides a manganese dioxide electrode material, a positive electrode sheet and a preparation method thereof.
[0005] The present invention adopts the following technical solution:
[0006] In a first aspect, a method for preparing a manganese dioxide electrode material is provided, which comprises the following steps:
[0007] (a) uniformly mixing potassium permanganate and divalent manganese salt in a predetermined ratio to obtain a precursor;
[0008] (b) ball milling the precursor obtained in step (a) in a ball mill for a predetermined time to obtain a ball-milled activated powder;
[0009] (c) heat treating the activated powder obtained in step (b) at 150-650° C. and then cooling to room temperature to obtain solid phase MnO2;
[0010] (d) uniformly mixing solid-phase MnO2 and aluminum salt solution in a predetermined ratio to obtain dispersed aluminum-doped solid-phase MnO2;
[0011] (e) After centrifugation, the aluminum-doped solid-phase MnO2 obtained in step (d) is washed with water until there are no impurity anions, and then dried to obtain the aluminum-doped solid-phase MnO2, that is, the manganese dioxide electrode material.
[0012] Preferably, in step (a), the divalent manganese salt is at least one of manganese carbonate, manganese chloride, manganese nitrate and manganese acetate.
[0013] Preferably, the divalent manganese salt is manganese carbonate.
[0014] Preferably, in step (a), the mass ratio of the potassium permanganate to the divalent manganese salt is 1:5 to 1:1.
[0015] Preferably, in step (b): the ball-to-material ratio is 1:1 to 10:1, preferably 1:1 to 7:1; the rotation speed of the ball mill is 500 to 10,000 rpm, and the ball milling time is 2 to 10 h; the ball milling medium is a non-metallic spherical ball, preferably a zirconia ball.
[0016] Preferably, the ball milling media are zirconia balls.
[0017] Preferably, in step (d), the mass ratio of the solid phase method MnO2 to the aluminum salt in the aluminum salt solution is 100:0.5 to 100:20.
[0018] Preferably, in step (d), the aluminum salt in the aluminum salt solution is at least one of aluminum chloride, aluminum sulfate and aluminum nitrate.
[0019] Preferably, in step (d), the solvent in the aluminum salt solution is water, ethanol or a mixture of the two.
[0020] Preferably, in step (d), the solvent in the aluminum salt solution is ethanol.
[0021] Preferably, in step (d), the aluminum salt solution has an aluminum salt concentration of 0.02 to 2 M
[0022] In a second aspect, a manganese dioxide electrode material prepared by the preparation method described in the first aspect is provided.
[0023] In the third aspect, a method for preparing a positive electrode sheet is provided, wherein the manganese dioxide electrode material prepared by the preparation method described in the first aspect is uniformly mixed with a conductive agent and a binder in a certain mass ratio, rolled to the surface of a conductive current collector, and dried to prepare a high-load positive electrode sheet.
[0024] Preferably, the mass ratio of manganese dioxide electrode material to conductive agent and binder is 6:3:1-8:1.5:0.5, the rolling pressure is 0.5-10 MPa, and the drying temperature is room temperature to 100°C.
[0025] In a fourth aspect, a positive electrode sheet prepared by the preparation method described in the third aspect is provided.
[0026] The present invention has the following advantages: the present invention mixes potassium permanganate and divalent manganese salt by ball milling and then roasts to obtain defect-rich α-MnO2, then realizes aluminum ion doping by solution exchange and then washes with water to obtain in-situ aluminum-doped solid-phase α-type manganese dioxide. The manganese dioxide electrode material prepared by the present invention can be applied to the positive electrode of electrochemical energy storage devices, for example, it can be applied to the positive electrode of aqueous primary and secondary batteries or supercapacitors, etc., which is beneficial to the stability of manganese dioxide during charging and discharging, and can effectively inhibit the dissolution of manganese dioxide positive electrodes, thereby improving the cycle stability of aqueous secondary batteries (such as). The manganese dioxide electrode material of the present invention can prepare a pole piece with high active component loading, large surface capacity and good cycle stability, and is particularly suitable for use as the positive electrode of aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The battery in the embodiment of the present invention and the control 1 is 0.1Ag -1 Cycling performance diagram under current density;
[0028] Figure 2 For the present invention example and control 2 at 0.5Ag -1 Cycling performance diagram at different current densities. DETAILED DESCRIPTION
[0029] The following is a detailed description of the embodiments of the present invention. It should be emphasized that the following description is only exemplary and is not intended to limit the scope and application of the present invention. In the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other.
[0030] The "room temperature" herein refers to 20-30°C.
[0031] A specific embodiment of the present invention provides a method for preparing a manganese dioxide electrode material, which comprises the following steps:
[0032] (a) potassium permanganate and a divalent manganese salt are uniformly mixed in a predetermined ratio to obtain a precursor; further: the divalent manganese salt is at least one of manganese carbonate, manganese chloride, manganese nitrate, and manganese acetate; the divalent manganese salt is preferably manganese carbonate; the mass ratio of the potassium permanganate to the divalent manganese salt is 1:5 to 1:1.
[0033] (b) ball milling the precursor obtained in step (a) for a predetermined time in a ball mill to obtain an activated powder after ball milling; further: the ball-to-material ratio during ball milling is 1:1-10:1, and more preferably the ball-to-material ratio is 1:1-7:1, the rotation speed of the ball mill is 500-10000 rpm, and the ball milling time is 2-10h; the ball milling medium is a non-metallic spherical ball, and more preferably the ball milling medium is a zirconia ball.
[0034] (c) heat treating the activated powder obtained in step (b) at 150-650°C and then cooling to room temperature to obtain solid phase MnO2; further: the heat treatment time is within 24 hours.
[0035] (d) The solid phase MnO2 and the aluminum salt solution are uniformly mixed in a predetermined proportion to obtain dispersed aluminum-doped solid phase MnO2; further: the mass ratio of the solid phase MnO2 to the aluminum salt in the aluminum salt solution is 100:0.5 to 100:20; the aluminum salt in the aluminum salt solution is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; the solvent in the aluminum salt solution is water, ethanol or a mixture of the two, more preferably ethanol; the concentration of the aluminum salt in the aluminum salt solution is 0.02 to 2M.
[0036] (e) The aluminum-doped solid-phase MnO2 of step (d) is centrifuged and washed with water until there is no impurity anion, and then dried to obtain the aluminum-doped solid-phase MnO2, that is, the manganese dioxide electrode material, and further: the drying temperature is room temperature to 200°C.
[0037] The specific embodiment of the present invention also provides a manganese dioxide electrode material prepared by the preparation method.
[0038] A specific embodiment of the present invention also provides a method for preparing a positive electrode sheet, which comprises uniformly mixing the manganese dioxide electrode material obtained by the preparation method with a conductive agent and a binder in a certain mass ratio, rolling the mixture to the surface of a conductive current collector, and drying the mixture to prepare a high-load positive electrode sheet; preferably, the mass ratio of the manganese dioxide electrode material to the conductive agent and the binder is 6:3:1 to 8:1.5:0.5, the rolling pressure is 0.5 to 10 MPa, and the drying temperature is room temperature to 100°C.
[0039] The specific embodiment of the present invention also provides a positive electrode sheet prepared by the preparation method.
[0040] The existing aluminum ion doped manganese dioxide preparation technology often requires high-temperature heat treatment, which causes the manganese dioxide to change phase and lose activity. Compared with the prior art, the manganese dioxide electrode material prepared in the specific embodiment of the present invention is aluminum ion doped solid phase method α-type manganese dioxide. Specifically, a high-capacity solid phase method α-type manganese dioxide is prepared by ball milling and low-temperature heat treatment. No wastewater is generated in the whole process. The preparation method is simple, environmentally friendly and energy-saving; the in-situ doping of aluminum ions is achieved by a solution adsorption method to prepare aluminum ion doped MnO2, and then in-situ reconstruction is carried out on the MnO2 surface during the water washing process (under the preparation method of the present invention, after aluminum ions are doped into the pores of manganese dioxide, under the action of H2O, the MnO2 structure is reconstructed, thereby generating aluminum doped solid phase method MnO2 (sometimes also referred to as boehmite-coated MnO2 in the specification and drawings of this article)), thereby improving the cycle stability of manganese dioxide in aqueous secondary batteries.
[0041] The specific embodiments of the present invention are further described below.
[0042] Example 1
[0043] Potassium permanganate and manganese carbonate were mixed in a mixer at a mass ratio of 1:1 for 1 hour, then transferred to a ball mill for 4 hours (ball-to-material ratio of 7:1, rotation speed of 1000 rpm), and then heat treated at 350°C in air atmosphere for 4 hours to obtain solid-phase MnO2.
[0044] Example 2
[0045] Potassium permanganate and manganese acetate were mixed in a mixer at a mass ratio of 1:1 for 1 hour, then transferred to a ball mill for 4 hours (ball-to-material ratio of 4:1, rotation speed of 1500 rpm), and then heat treated at 350°C in air atmosphere for 4 hours to obtain solid-phase MnO2.
[0046] Example 3
[0047] Potassium permanganate and manganese chloride were mixed in a mixer at a mass ratio of 1:1 for 1 hour, then transferred to a ball mill for 4 hours (ball-to-material ratio of 10:1, rotation speed of 2000 rpm), and then heat treated at 350°C in air atmosphere for 4 hours to obtain solid-phase MnO2.
[0048] Example 4
[0049] The solid phase method MnO2 prepared in Example 1 was uniformly mixed with 0.5M aluminum chloride ethanol solution (the mass of aluminum chloride was 10wt.% of MnO2) for 2h, and then centrifuged to obtain an aluminum ion-doped solid phase method MnO2 containing ethanol sample, and the separated aluminum chloride ethanol solution was used for the next experiment. The solid phase method MnO2 containing ethanol sample was washed with deionized water for 3 times until there was no impurity anion, and dried at 100°C for 4h to obtain aluminum-doped solid phase method MnO2.
[0050] Example 5
[0051] The solid phase method MnO2 prepared in Example 1 was uniformly mixed with 0.5M aluminum sulfate aqueous solution (the mass of aluminum sulfate was 10wt.% of MnO2) for 2h, and then centrifuged to obtain an aluminum ion-doped solid phase method MnO2 aqueous sample, and the separated aluminum sulfate aqueous solution was used for the next experiment. The aluminum ion-doped solid phase method MnO2 aqueous sample was washed with deionized water 3 times and dried at 100°C for 4h to obtain aluminum-doped solid phase method MnO2.
[0052] Example 6
[0053] The solid phase method MnO2 prepared in Example 1 was uniformly mixed with 0.5M aluminum nitrate ethanol solution (the mass of aluminum nitrate was 10wt.% of MnO2) for 2h, and then centrifuged to obtain an aluminum ion-doped solid phase method MnO2 containing ethanol sample, and the separated aluminum nitrate ethanol solution was used for the next experiment. The aluminum ion-doped solid phase method MnO2 containing ethanol sample was washed 3 times with deionized water and dried at 100°C for 4h to obtain aluminum-doped solid phase method MnO2.
[0054] Preparation of the battery in this example: A manganese dioxide-zinc full battery was assembled according to the positive electrode (manganese dioxide (aluminum-doped solid-phase MnO2 prepared in Example 4): binder (PTFE): conductive agent (carbon black) = 7:1:2): zinc foil negative electrode capacity ratio of 1:3; the separator was a commercial glass fiber membrane; the electrolyte was 2MZnSO4+0.2M MnSO4 solution. Performance characterization CR2025 button battery, using Blue Electric CT3001A, at 0.1Ag -1 and 0.5Ag -1 Performance test at current density.
[0055] As a control for the above battery, control 1: The difference from the battery of the present embodiment is that the manganese dioxide in the positive electrode is MnO2 prepared by the solid phase method in Example 1. Control 2: The difference from the battery of the present embodiment is that 2MZnSO4 is used as the electrolyte.
[0056] like Figure 1 The following are the manganese dioxide prepared by different methods ( Figure 1 In the table, “solid-phase MnO2” refers to the solid-phase MnO2 prepared in Example 1, and “boehmite-coated solid-phase MnO2” refers to the aluminum-doped solid-phase MnO2 prepared in Example 4. -2 , charge and discharge current density 0.1A·g -1 ), it can be seen that the cycle performance of the aluminum-doped manganese dioxide in the embodiment of the present invention is much better than the cycle performance of the manganese dioxide not doped with aluminum.
[0057] like Figure 2 As shown, the capacity comparison of aluminum-doped solid-phase manganese dioxide in different electrolyte systems (positive electrode surface loading 17±0.5mg·cm -2 , charge and discharge current density 0.5A·g -1 ), it can be seen that aluminum-doped solid-phase manganese dioxide can still operate stably in an electrolyte without MnSO4, although the capacity is relatively small.
[0058] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, it can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A method for preparing a manganese dioxide electrode material, characterized in that: The steps include: (a) uniformly mixing potassium permanganate and divalent manganese salt in a predetermined ratio to obtain a precursor; (b) ball milling the precursor obtained in step (a) in a ball mill for a predetermined time to obtain a ball-milled activated powder; (c) heat treating the activated powder obtained in step (b) at 150-650° C. and then cooling to room temperature to obtain solid phase MnO2; (d) uniformly mixing solid-phase MnO2 and aluminum salt solution in a predetermined ratio to obtain dispersed aluminum-doped solid-phase MnO2; (e) After centrifugation, the aluminum-doped solid-phase MnO2 obtained in step (d) is washed with water until there are no impurity anions, and then dried to obtain the aluminum-doped solid-phase MnO2, that is, the manganese dioxide electrode material.
2. The preparation method according to claim 1, characterized in that: In step (a), the divalent manganese salt is at least one of manganese carbonate, manganese chloride, manganese nitrate and manganese acetate; the divalent manganese salt is preferably manganese carbonate.
3. The preparation method according to claim 1, characterized in that: In step (a), the mass ratio of the potassium permanganate to the divalent manganese salt is 1:5 to 1:
1.
4. The preparation method according to claim 1, characterized in that: In step (b), the ball-to-material ratio is 1:1 to 10:1, preferably 1:1 to 7:1; the rotation speed of the ball mill is 500 to 10,000 rpm, and the ball milling time is 2 to 10 hours; the ball milling medium is a non-metallic sphere, preferably a zirconia ball.
5. The preparation method according to claim 1, characterized in that: In step (d), the mass ratio of the solid phase method MnO2 to the aluminum salt in the aluminum salt solution is 100:0.5 to 100:
20.
6. The preparation method according to claim 1, characterized in that: In step (d), the aluminum salt in the aluminum salt solution is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; in step (d), the solvent in the aluminum salt solution is water, ethanol, or a mixture of the two, preferably ethanol; in the aluminum salt solution, the aluminum salt concentration is 0.02 to 2M.
7. A manganese dioxide electrode material prepared by the preparation method according to any one of claims 1 to 6.
8. A method for preparing a positive electrode sheet, characterized in that: The manganese dioxide electrode material prepared by the preparation method according to any one of claims 1 to 6 is uniformly mixed with a conductive agent and a binder in a certain mass ratio, rolled to the surface of a conductive current collector, and dried to prepare a high-load positive electrode sheet; preferably, the mass ratio of the manganese dioxide electrode material to the conductive agent and the binder is: 6:3:1-8:1.5:0.5, the rolling pressure is 0.5-10MPa, and the drying temperature is room temperature to 100°C.
9. A positive electrode sheet obtained by the preparation method of claim 8.