Capacitive deionization negative electrode, capacitive deionization positive electrode, processing method of capacitive deionization negative electrode and capacitive deionization device
By using sulfuric acid or ammonium sulfate solution and ammonia water to treat the capacitance deionized pole sheet, the ion adsorption performance of the capacitance deionized device is improved, and the problems of high cost and low desalination rate in the prior art are solved, thereby achieving efficient ion Removal effect, suitable for household water purification equipment.
Patent Information
- Application Number
- CN202411278658.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing electrochemical deionization technology, the ion exchange membrane is costly and prone to breed bacteria, resulting in low desalination rate and cannot meet users' needs for mineral water and purified water at the same time.
Use sulfuric acid or ammonium sulfate solution to treat the capacitance deionized electrode sheet to oxidize the surface groups of the active material to improve the ion adsorption performance; use ammonia water or polyethylene polyamine aqueous solution to treat the capacitance deionized electrode sheet to increase amino or ammonium ions and improve the anion Adsorption capacity.
It significantly improves the ion adsorption amount and removal efficiency of capacitor deionized devices, reduces costs, and is suitable as a household water purification equipment for residents.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water treatment, and in particular to a capacitor deionization negative electrode, a positive electrode and a treatment method thereof, and a capacitor deionization device. Background Art
[0002] Most household water purification equipment is based on RO membranes, which are non-selective and have a desalination rate of over 90%. With people's demand for healthy living, water purifiers with the function of retaining minerals are a new trend. Electrochemical deionization technology can effectively achieve adjustable desalination rate.
[0003] However, most electrochemical schemes require ion exchange membranes, such as electrodialysis technology and membrane capacitor deionization technology. Ion exchange membranes have high costs and are prone to breeding bacteria after long-term operation, which is not conducive to use by ordinary users. Capacitor deionization technology without ion exchange membranes has a low desalination rate and cannot meet the needs of users for mineral water and pure water at the same time. Therefore, developing a capacitor deionization module electrode with a high adsorption capacity to improve the desalination rate of the device can effectively promote the application and promotion of capacitor deionization technology in ordinary users' homes. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the prior art at least to a certain extent. To this end, one object of the present invention is to provide a capacitor deionization negative electrode, a positive electrode and a processing method thereof and a capacitor deionization device.
[0005] In a first aspect of the present invention, the present invention provides a method for treating a negative electrode of a capacitor deionizer. According to an embodiment of the present invention, the method comprises: The capacitor deionization electrode is brought into contact with a first solution to react, wherein the first solution includes a sulfuric acid solution and / or an ammonium sulfate solution.
[0006] According to the treatment method of the capacitor deionization negative electrode of the above embodiment of the present invention, the capacitor deionization electrode is contacted with the first solution to react, and the first solution includes a sulfuric acid solution and / or an ammonium sulfate solution. The inventor found that the capacitor deionization electrode is treated with a sulfuric acid solution and / or an ammonium sulfate solution. The first solution with strong oxidizing property can oxidize the surface group of the carbon material (activated carbon) in the active material layer of the electrode to -COOH, and can also oxidize the -OH of the binder in the active material layer of the electrode to -COOH, or oxidize to form some other active groups, thereby significantly improving the ion adsorption performance of the electrode, and after the reaction, sulfonic acid groups will be grafted in the active material layer of the electrode. At the same time, under the action of the first solution, the surface of the electrode may also undergo some microscopic changes. The grafting of sulfonic acid groups and the microscopic changes in the structure can both enhance the selective adsorption of ions, thereby significantly increasing the amount of ion adsorption. Therefore, the treatment method is simple in process, does not require expensive equipment investment, and the reagents used are cheap and easy to obtain, and the cost is low. The use of this treatment method for commercially available or finished electrode pieces can significantly increase the ion adsorption of the electrode piece and improve the ion removal efficiency, providing a new idea for improving the performance of capacitor deionization devices.
[0007] In addition, the method for treating the negative electrode of capacitor deionization according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, the mass concentration of the first solution is 0.1%~50%.
[0008] In some embodiments of the present invention, the mass concentration of the first solution is 1% to 20%.
[0009] In some embodiments of the present invention, the amount of the first solution applied to the capacitor deionization electrode is 3 mg / cm 2 ~10mg / cm 2 .
[0010] In some embodiments of the present invention, the contacting manner includes immersion, scraping, spin coating, dip coating or spray coating.
[0011] In some embodiments of the present invention, the temperature for the capacitor deionization electrode to contact with the first solution to react is 0° C. to 200° C. and the time is 0.5 h to 100 h.
[0012] In some embodiments of the present invention, the temperature for reacting the capacitor deionization electrode with the first solution is 40° C. to 100° C., and the time is 0.5 h to 2 h.
[0013] In the second aspect of the present invention, the inventors propose a capacitor deionization negative electrode. According to an embodiment of the present invention, the capacitor deionization negative electrode is obtained by processing using the above method. Thus, the capacitor deionization negative electrode has a large ion adsorption capacity and high ion removal efficiency.
[0014] In a third aspect of the present invention, the present invention provides a method for treating a positive electrode of a capacitor deionizer. According to an embodiment of the present invention, the method comprises: The capacitor deionization electrode is brought into contact with a second solution to react, wherein the second solution includes ammonia water and / or polyethylene polyamine aqueous solution.
[0015] According to the treatment method of the positive electrode of the capacitor deionization of the above embodiment of the present invention, the capacitor deionization electrode is contacted with the second solution to react, and the second solution includes ammonia water and / or polyethylene polyamine aqueous solution. The inventor found that the capacitor deionization electrode is treated with the second solution. On the one hand, under the action of ammonia water or the dehydration process of polyethylene polyamine, the amino group may be grafted into the carbon material (activated carbon) in the electrode active material layer, so that the electrode has high selectivity for anions and increases the adsorption amount; on the other hand, the amino group or ammonium ion is adsorbed on the surface of the active material layer of the electrode, forming a positive charge on the electrode surface, repelling cations, and having an adsorption effect on anions. Or under the action of ammonia water or polyethylene polyamine, the surface of the electrode may also undergo some microscopic changes, and these microscopic changes will also increase the adsorption effect of the electrode. Therefore, the treatment method is simple in process, does not require expensive equipment investment, and the reagents used are cheap and easy to obtain, and the cost is low. The treatment method is used for commercially available or finished electrode pieces, which can significantly increase the ion adsorption amount of the electrode piece and improve the ion removal efficiency, providing a new idea for improving the performance of capacitor deionization devices.
[0016] In addition, the method for processing the positive electrode of capacitor deionization according to the above embodiment of the present invention also has the following technical features: In some embodiments of the present invention, the mass concentration of the ammonia water is 0.1%~28%.
[0017] In some embodiments of the present invention, the mass concentration of the polyethylene polyamine aqueous solution is not less than 90%.
[0018] In some embodiments of the present invention, the contacting manner includes immersion, scraping, spin coating, dip coating or spray coating.
[0019] In some embodiments of the present invention, the temperature for the capacitor deionization electrode to contact with the second solution for reaction is 20° C. to 150° C., the time is 0.5 h to 100 h, and the pressure is 0.1 MPa to 5 MPa.
[0020] In some embodiments of the present invention, the temperature for the capacitor deionization electrode to contact the second solution for reaction is 80° C. to 150° C., the time is 0.5 h to 8 h, and the pressure is 0.1 MPa to 0.2 MPa.
[0021] In a fourth aspect of the present invention, the present invention provides a capacitor deionization positive electrode. According to an embodiment of the present invention, the capacitor deionization positive electrode is obtained by processing using the above method. Thus, the capacitor deionization positive electrode has a large ion adsorption capacity and high ion removal efficiency.
[0022] In a fifth aspect of the present invention, the present invention provides a capacitor deionization device. According to an embodiment of the present invention, the capacitor deionization device includes the above-mentioned capacitor deionization positive electrode and / or the above-mentioned capacitor deionization negative electrode. As a result, the capacitor deionization device has a large adsorption capacity and high ion removal efficiency, and is suitable as a household water purification device. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In a first aspect of the present invention, the present invention provides a method for treating a negative electrode of a capacitor deionizer. According to an embodiment of the present invention, the method comprises: The capacitor deionization electrode is brought into contact with a first solution to react, wherein the first solution includes a sulfuric acid solution and / or an ammonium sulfate solution.
[0025] According to the treatment method of the capacitor deionization negative electrode of the above embodiment of the present invention, the capacitor deionization electrode is contacted with the first solution to react, and the first solution includes a sulfuric acid solution and / or an ammonium sulfate solution. The inventor found that the capacitor deionization electrode is treated with a sulfuric acid solution and / or an ammonium sulfate solution. The first solution with strong oxidizing property can oxidize the surface group of the carbon material (activated carbon) in the active material layer of the electrode to -COOH, and can also oxidize the -OH of the binder in the active material layer of the electrode to -COOH, or oxidize to form some other active groups, thereby significantly improving the ion adsorption performance of the electrode, and after the reaction, sulfonic acid groups will be grafted in the active material layer of the electrode. At the same time, under the action of the first solution, the surface of the electrode may also undergo some microscopic changes. The grafting of sulfonic acid groups and the microscopic changes in the structure can both enhance the selective adsorption of ions, thereby significantly increasing the amount of ion adsorption. Therefore, the treatment method is simple in process, does not require expensive equipment investment, and the reagents used are cheap and easy to obtain, and the cost is low. The use of this treatment method for commercially available or finished electrode pieces can significantly increase the ion adsorption of the electrode piece and improve the ion removal efficiency, providing a new idea for improving the performance of capacitor deionization devices.
[0026] It should be noted that the capacitor deionization electrode is a commercially available electrode that can be used directly or a conventional electrode prepared by an existing method. The above method of the present application is applicable to all existing capacitor deionization electrodes.
[0027] As an example, activated carbon, conductive carbon black and a binder are weighed and mixed in a certain mass ratio. After mixing, the solid powder is added to a solvent to form a mixed solution with a certain solid content. After stirring with a stirrer, a uniform slurry is formed. A coating device is used to coat the slurry on the current collector. After drying and rolling, a conventional electrode is formed.
[0028] The above-mentioned activated carbon, conductive carbon black, binder, and current collector are all conventional materials in the art and are not particularly limited here.
[0029] According to an embodiment of the present invention, the mass concentration of the first solution is 0.1% to 50%, preferably 1% to 20%. For example, the mass concentration of the first solution is 0.1%, 0.5%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, etc., and the mass concentration is greater than or equal to 0.1%, 0.5%, 1%, 5%, 10%, etc., and less than or equal to 20%, 30%, 40%, 50%, etc. The inventors found that the mass concentration of the first solution is too low to oxidize the electrode, but the mass concentration of the first solution is too high, and the oxidizing property of the first solution is too strong. During the coating process, the first solution quickly oxidizes the electrode components, causing the active material layer and the current collector to fall off. It should be noted that when the mass concentration of the first solution is small, drying occurs spontaneously first, the concentration of the acid increases, and then reacts with the active material layer of the electrode.
[0030] According to an embodiment of the present invention, the amount of the first solution applied to the capacitor deionization electrode is 3 mg / cm 2 ~10mg / cm 2 For example, the application amount is 3mg / cm 2 , 4mg / cm 2 , 5mg / cm 2 , 6mg / cm 2 , 7mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 , 10mg / cm 2 For example, the applied amount is greater than or equal to 3mg / cm 2 , 4mg / cm 2 , 5mg / cm 2 , 6mg / cm 2 Etc., less than or equal to 7mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 , 10mg / cm2 By controlling the amount of the first solution applied to the capacitor deionization electrode to be 3 mg / cm 2 ~10mg / cm 2 , the first solution can fully react with the active material layer of the electrode, thereby increasing the adsorption capacity of the electrode. It should be noted that the applied amount refers to the mass of the first solution per unit area of the active material layer of the electrode.
[0031] According to an embodiment of the present invention, the contacting method includes immersion, scraping, spin coating, dipping or spraying, preferably scraping, spin coating, dipping or spraying.
[0032] As an example, soaking refers to immersing the capacitor deionization electrode into the first solution, but the inventors have found that if the soaking time is too long, the current collector of the electrode may be separated from the active material layer. Therefore, those skilled in the art can select the soaking time according to actual conditions.
[0033] As an example, the scraping method refers to scraping the first solution onto the surface of the active material layer of the capacitor deionization electrode to fully wet the active material layer.
[0034] As an example, dip coating is to put the capacitor deionization electrode into the first solution and then take it out, that is, the first solution is attached to the surface of the electrode.
[0035] According to an embodiment of the present invention, the temperature for the capacitor deionization electrode to contact and react with the first solution is 0°C~200°C, preferably 40°C~100°C, for example, the temperature is greater than or equal to 0°C, 10°C, 30°C, 50°C, etc., and less than or equal to 200°C, 150°C, 120°C, 100°C, 80°C, 60°C, etc.; the time is 0.5h~100h, preferably 0.5h~2h, for example, the time is greater than or equal to 0.5h, 1h, 2h, 5h, 10h, etc., and less than or equal to 100h, 80h, 50h, 30h, 10h, etc. The inventors have found that controlling the temperature for the capacitor deionization electrode to contact and react with the first solution to be 0°C~200°C and the time to be 0.5h~100h can make the capacitor deionization electrode contact and react fully with the first solution, thereby improving the adsorption performance of the capacitor deionization negative electrode.
[0036] According to an embodiment of the present invention, after the contact reaction between the capacitor deionization electrode and the first solution is completed, the electrode is cleaned with water or deionized water to remove the unreacted first solution.
[0037] In the second aspect of the present invention, the inventors propose a capacitor deionization negative electrode. According to an embodiment of the present invention, the capacitor deionization negative electrode is obtained by processing using the above method. As a result, the capacitor deionization negative electrode has a large ion adsorption capacity and a high ion removal efficiency. It should be noted that the features and advantages described in the above processing method for the capacitor deionization negative electrode are also applicable to the capacitor deionization negative electrode, and will not be repeated here.
[0038] In a third aspect of the present invention, the present invention provides a method for treating a positive electrode of a capacitor deionizer. According to an embodiment of the present invention, the method comprises: The capacitor deionization electrode is brought into contact with a second solution to react, wherein the second solution includes ammonia water and / or polyethylene polyamine aqueous solution.
[0039] According to the treatment method of the positive electrode of the capacitor deionization of the above embodiment of the present invention, the capacitor deionization electrode is contacted with the second solution to react, and the second solution includes ammonia water and / or polyethylene polyamine aqueous solution. The inventor found that the capacitor deionization electrode is treated with the second solution. On the one hand, under the action of ammonia water or the dehydration process of polyethylene polyamine, the amino group may be grafted into the carbon material (activated carbon) in the electrode active material layer, so that the electrode has high selectivity for anions and increases the adsorption amount; on the other hand, the amino group or ammonium ion is adsorbed on the surface of the active material layer of the electrode, forming a positive charge on the electrode surface, repelling cations, and having an adsorption effect on anions. Or under the action of ammonia water or polyethylene polyamine, the surface of the electrode may also undergo some microscopic changes, and these microscopic changes will also increase the adsorption effect of the electrode. Therefore, the treatment method is simple in process, does not require expensive equipment investment, and the reagents used are cheap and easy to obtain, and the cost is low. The treatment method is used for commercially available or finished electrode pieces, which can significantly increase the ion adsorption amount of the electrode piece and improve the ion removal efficiency, providing a new idea for improving the performance of capacitor deionization devices.
[0040] It should be noted that the capacitor deionization electrode is a commercially available electrode that can be used directly or a conventional electrode prepared by an existing method. The above method of the present application is applicable to all existing capacitor deionization electrodes.
[0041] As an example, activated carbon, conductive carbon black and a binder are weighed and mixed in a certain mass ratio. After mixing, the solid powder is added to a solvent to form a mixed solution with a certain solid content. After stirring with a stirrer, a uniform slurry is formed. A coating device is used to coat the slurry on the current collector. After drying and rolling, a conventional electrode is formed.
[0042] The above-mentioned activated carbon, conductive carbon black, binder, and current collector are all conventional materials in the art and are not particularly limited here.
[0043] According to an embodiment of the present invention, the mass concentration of the ammonia water is 0.1% to 28%. For example, the mass concentration of the ammonia water is 0.1%, 1%, 3%, 6%, 10%, 15%, 20%, 28%, etc., and the mass concentration is greater than or equal to 0.1%, 1%, 3%, 6%, etc., and less than or equal to 10%, 15%, 20%, 28%, etc. The inventors have found that when the mass concentration of the ammonia water is controlled within the range of 0.1% to 28%, the ammonia water can fully react with the active material layer of the electrode, thereby improving the adsorption performance of the capacitor deionization positive electrode.
[0044] According to an embodiment of the present invention, the mass concentration of the polyethylene polyamine aqueous solution is not less than 90%. For example, the mass concentration is 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, etc. The inventors have found that the mass concentration of the polyethylene polyamine aqueous solution is not less than 90%, which can fully react with the active material layer of the electrode sheet, thereby improving the adsorption performance of the capacitor deionization positive electrode.
[0045] According to an embodiment of the present invention, the contacting manner includes immersion, scraping, spin coating, dip coating or spray coating.
[0046] According to an embodiment of the present invention, the temperature for contacting the capacitor deionization electrode with the second solution to react is 20°C~150°C, preferably 80°C~150°C, for example, the temperature is greater than or equal to 20°C, 30°C, 40°C, 50°C, etc., and less than or equal to 150°C, 130°C, 110°C, 80°C, 60°C, etc.; the time is 0.5h~100h, preferably 0.5h~8h, for example, the time is greater than or equal to 0.5h, 1h, 3h, 10h, 20h, etc., and less than or equal to 100h, 90h, 70h, 50h, 30h, etc.; the pressure is 0.1MPa~5MPa, preferably 0.1MPa~0.2MPa, for example, the pressure is greater than or equal to 0.1MPa, 1MPa, 2MPa, etc., and less than or equal to 3MPa, 4MPa, 5MPa, etc. The inventors have found that by controlling the temperature of the capacitor deionization electrode and the second solution to react at 20°C~150°C, the time to 0.5h~100h, and the pressure to 0.1MPa~5MPa, the capacitor deionization electrode and the second solution can be fully reacted in contact, thereby improving the adsorption performance of the capacitor deionization positive electrode. In particular, because ammonia itself has a certain volatility, controlling the reaction pressure within the range of 0.1MPa~5MPa can improve the reaction efficiency.
[0047] According to an embodiment of the present invention, after the contact reaction between the capacitor deionization electrode and the second solution is completed, the electrode is cleaned with water or deionized water to remove the unreacted second solution.
[0048] In a fourth aspect of the present invention, the present invention proposes a capacitor deionization positive electrode. According to an embodiment of the present invention, the capacitor deionization positive electrode is obtained by processing using the above method. As a result, the capacitor deionization positive electrode has a large ion adsorption capacity and a high ion removal efficiency. It should be noted that the features and advantages described in the above processing method for the capacitor deionization positive electrode are also applicable to the capacitor deionization positive electrode, and will not be repeated here.
[0049] In a fifth aspect of the present invention, the present invention provides a capacitor deionization device. According to an embodiment of the present invention, the capacitor deionization device includes the above-mentioned capacitor deionization positive electrode and / or the above-mentioned capacitor deionization negative electrode. As a result, the capacitor deionization device has a large adsorption capacity and high ion removal efficiency, and is suitable as a household water purification device.
[0050] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0051] The commercially available capacitor deionization electrode was obtained from Chongqing Zhongke Chaocapacitor Technology Co., Ltd. The commercially available capacitor deionization electrode used in the examples and comparative examples of the present application is the same.
[0052] Capacitor deionized negative electrode A: A commercially available capacitor deionized electrode was treated in situ with a sulfuric acid solution having a mass concentration of 1%. Specifically, the sulfuric acid solution was coated on the surface of the electrode, the application amount was 10 mg / cm2, the standing temperature range was 50°C, the standing time was 1 hour, and after the standing period, the electrode was washed 5 times with deionized water.
[0053] Capacitor deionization negative electrode B: A commercially available capacitor deionization electrode was treated in situ with a sulfuric acid solution having a mass concentration of 20%. Specifically, the sulfuric acid solution was coated on the surface of the electrode, the application amount was 5 mg / cm2, the standing temperature range was 50°C, the standing time was 1 hour, and after the standing period, the electrode was washed 5 times with deionized water.
[0054] Capacitor deionization negative electrode C: A commercially available capacitor deionization electrode was treated in situ with a sulfuric acid solution having a mass concentration of 40%. Specifically, the sulfuric acid solution was coated on the surface of the electrode, the application amount was 3 mg / cm2, the standing temperature range was 50°C, the standing time was 1 hour, and after the standing period, the electrode was washed 5 times with deionized water.
[0055] When a commercially available capacitor deionization electrode is treated in situ with a sulfuric acid solution having a mass concentration of 60%, the current collector and active material layer of the electrode are separated.
[0056] Capacitor deionization negative electrode D: A commercially available capacitor deionization electrode was treated in situ with an ammonium sulfate solution having a mass concentration of 20%. Specifically, the ammonium sulfate solution was coated on the surface of the electrode, the application amount was 10 mg / cm2, the standing temperature range was 50°C, the standing time was 1 hour, and after the standing period, the electrode was washed 5 times with deionized water.
[0057] Capacitor deionized positive electrode A: A commercially available capacitor deionized electrode was treated in situ with ammonia water having a mass concentration of 10%. Specifically, the ammonia water was coated on the surface of the electrode and allowed to stand at a temperature of 80°C for 2 hours and a pressure of 0.2MPa. After the standing period, the electrode was washed 5 times with deionized water.
[0058] Capacitor deionized positive electrode B: A commercially available capacitor deionized electrode was treated in situ with a polyethylene polyamine solution having a mass concentration of 98%. Specifically, the polyethylene polyamine solution was coated on the surface of the electrode and allowed to stand at a temperature of 80°C for 2 hours and a pressure of 0.2 MPa. After the standing period, the electrode was washed 5 times with deionized water.
[0059] The examples and comparative examples use the negative electrode or positive electrode prepared as described above, as shown in Table 1.
[0060] The performance of the capacitive deionization devices prepared in the examples and comparative examples was tested, and the specific testing method was as follows: The positive electrode-mesh-negative electrode-mesh are arranged alternately to prepare a plate-shaped or rolled capacitive deionization module. The adsorption process: the inlet water flow rate and the total electrode area maintain a relationship of 0.5 L / min·m2, the positive electrode is connected to positive electricity, and the negative electrode is connected to negative electricity. Ions in water are adsorbed. The inlet water concentration is 200ppm aqueous solution, the positive and negative electrode voltages are 1.5V, the outlet water TDS is tested, and the adsorption amount per unit area per unit time is calculated accordingly.
[0061] The performance test results of the capacitive deionization devices prepared in the examples and comparative examples are shown in Table 1.
[0062] Table 1
[0063] From the data in Table 1, it can be seen that the sulfonated negative electrode or the aminated positive electrode can increase the ion adsorption capacity of the electrode. After the positive and negative electrodes are treated at the same time, the adsorption capacity of the electrodeionization system can be increased by more than 1 times.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for treating a negative electrode of a capacitor deionization, characterized in that: include: The capacitor deionization electrode is brought into contact with a first solution to react, wherein the first solution includes a sulfuric acid solution and / or an ammonium sulfate solution.
2. The method according to claim 1, characterized in that: The mass concentration of the first solution is 0.1% to 50%, preferably 1% to 20%.
3. The method according to claim 1 or 2, characterized in that: The amount of the first solution applied to the capacitor deionization electrode is 3 mg / cm 2 ~10mg / cm 2 ; And / or, the contacting method includes immersion, scraping, spin coating, dip coating or spray coating.
4. The method according to claim 1 or 2, characterized in that: The temperature for the capacitor deionization electrode to contact with the first solution for reaction is 0°C to 200°C, preferably 40°C to 100°C, and the time is 0.5h to 100h, preferably 0.5h to 2h.
5. A capacitor deionization negative electrode, characterized in that: The product is obtained by processing according to any one of claims 1 to 4.
6. A method for treating a positive electrode of a capacitor deionizer, characterized in that: include: The capacitor deionization electrode is brought into contact with a second solution to react, wherein the second solution includes ammonia water and / or polyethylene polyamine aqueous solution.
7. The method according to claim 6, characterized in that: The mass concentration of the ammonia water is 0.1%~28%; and / or, the mass concentration of the polyethylene polyamine aqueous solution is not less than 90%; And / or, the contacting method includes immersion, scraping, spin coating, dip coating or spray coating.
8. The method according to claim 6, characterized in that: The temperature for contacting the capacitor deionization electrode with the second solution to react is 20°C to 150°C, preferably 80°C to 150°C, the time is 0.5h to 100h, preferably 0.5h to 8h, and the pressure is 0.1MPa to 5MPa, preferably 0.1MPa to 0.2MPa.
9. A capacitor deionization positive electrode, characterized in that: The method is used to obtain the product according to any one of claims 6 to 8.
10. A capacitive deionization device, characterized in that: It comprises the capacitor deionization negative electrode as described in claim 5 and / or the capacitor deionization positive electrode as described in claim 9.
Citation Information
Patent Citations
Graphene / NiO nanocomposite aerogel capacitor desalting electrode and preparation method thereof
CN107140717A
Composite material for removing heavy metal ions in water
CN110302767A
Flow electrode and application thereof
CN110372067A
Method for selective separation of ionic species from ionic solution based on ionic hydrated size
US20210331947A1
Method for selective separation of monovalent ionic species using electrodes functionalized with sulfonic groups
US20220064029A1
Cited By
Capacitive deionization negative electrode and positive electrode, treatment methods therefor, and capacitive deionization device
WO2026056870A1