Transition metal ion doped colored fused quartz glass and preparation method thereof
Through photocuring technology and heat treatment optimization, the problem of cracking and crystallization of fused quartz glass during degreasing and sintering was solved, and doped transition metal ionic non-colored fused quartz glass with high light transmittance and optical properties was prepared, suitable for Complex shapes and multifunctional optics.
Patent Information
- Application Number
- CN202410983137.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing preparation methods for colored fused quartz glass have cracked or severe crystallization due to factors such as degreasing and inappropriate sintering heat treatment process.
Photocuring technology is used to disperse SiO2 powder in photosensitive resin to print into a three-dimensional glass embryo. The degreasing conditions are determined through thermal gravity and differential scanning calorimetry test, degreasing heat treatment is performed, and ion doping is performed at a specific temperature and time. By sintering treatment, colored fused quartz glass doped with transition metal ions is prepared.
The prepared glass has high light transmittance, good elastic modulus and hardness, maintains an amorphous state, and can adjust the absorption capacity of light in different bands, expanding its application in optical devices and other fields.
Smart Images

Figure CN118908544A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical elements, and in particular to colored fused quartz glass doped with transition metal ions and a preparation method thereof. Background Art
[0002] Fused quartz glass is widely used in scientific research, industrial development and social production. Its superior optical transparency, thermal stability, chemical stability and mechanical stability make it an irreplaceable material. However, its high melting temperature and hard and brittle characteristics make traditional hot forming preparation technology and machining difficult, limiting the use of fused quartz glass. 3D printing to prepare fused quartz glass has significant advantages in manufacturing parts with complex shapes, and has become an ideal technology for manufacturing fused quartz glass parts in recent years. 3D printing to prepare glass mainly focuses on two directions. Direct additive manufacturing directly 3D prints low-melting point glass at high temperature; indirect additive manufacturing technology prints fused quartz glass precursors, and then performs two-step heat treatment of degreasing and sintering to remove organic matter and densify SiO2 powder to obtain transparent fused quartz glass. However, the processing accuracy and surface quality of direct additive manufacturing are poor, and further post-processing is required.
[0003] At present, the indirect additive manufacturing methods for fused silica glass that are widely studied mainly include photolithography, ink direct writing and sol-gel. Compared with ink direct writing and sol-gel, photolithography does not require drying and dehydration, and the preparation cycle is short. In addition, the glass prepared by photolithography has high molding precision, good surface quality and excellent mechanical properties. At the same time, the actual application time of photolithography is early and the process is mature. Photolithography has high printing precision, fast speed and good surface quality, and has great application potential in the preparation of flow channel structures, optical lenses and handicrafts. However, fused silica glass parts not only require complex geometric shapes, but also need to have diverse optical properties. The optical absorption characteristics, photoluminescence characteristics and light scattering characteristics of glass can be changed by metal ion doping. Among metal elements, the electronic state of the d orbit of transition metal elements is relatively rich, and the emission range of dd transition is very wide, so it has different uses. Glass doped with transition metal elements Cr and Co has certain applications in integrated optical devices, filters, visible light and near-infrared laser materials. However, during the preparation process, fused quartz glass doped with transition metal elements often suffers from cracking or severe crystallization problems after heat treatment due to factors such as excessive element concentration, inappropriate temperature during degreasing and sintering heat treatment processes. Therefore, a method for improving the quality of fused quartz glass doped with transition metal elements is urgently needed. Summary of the invention
[0004] The technical problems to be solved by the present invention are:
[0005] The existing method for preparing colored fused quartz glass often causes the colored fused quartz glass to crack or seriously devitrify due to factors such as inappropriate temperatures during degreasing and sintering heat treatment processes.
[0006] The present invention adopts the following technical solutions to solve the above technical problems:
[0007] The present invention provides a method for preparing colored fused quartz glass doped with transition metal ions, comprising the following steps:
[0008] S1, prepare photosensitive resin, disperse SiO2 powder in the photosensitive resin to obtain photosensitive slurry;
[0009] S2, using light-curing technology to print the photosensitive slurry to form a three-dimensional glass embryo;
[0010] S3, performing thermogravimetric and differential scanning calorimetry tests on the glass embryo, and constructing thermogravimetric and differential scanning calorimetry data curves during the construction process;
[0011] S4, determining the degreasing conditions according to the thermogravimetric and differential scanning calorimetry data curves, and performing degreasing heat treatment on the glass embryo;
[0012] S5, placing the degreased parts in a transition metal ion solution for ion doping, and drying;
[0013] S6. Perform a thermal expansion test on the degreased part after doping to determine the sintering conditions, and perform a sintering treatment on the degreased part after doping to obtain the colored glass doped with transition metal ions.
[0014] Furthermore, the mass ratio of the photosensitive resin to SiO2 in S1 is 47:53.
[0015] Further, the photosensitive resin in S1 includes, by mass, 100 parts of a photosensitive monomer, 0.2 parts of diethyl phthalate, 0.5 parts of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and 0.05 parts of Sudan Orange G;
[0016] The photosensitive monomers include, by mass, 60.8 parts of hydroxyethyl acrylate, 8.3 parts of monomer triethylene glycol diacrylate and 30.9 parts of phenoxyethanol.
[0017] Furthermore, the degreasing conditions in S4 are: heating at 220° C. for 2 hours, 340° C. for 4 hours and 600° C. for 2 hours in an air atmosphere by a programmed temperature increase method.
[0018] Furthermore, the specific process of the degreasing heat treatment described in S4 is: in an air atmosphere, the temperature is increased by a programmed temperature rising method at 24°C per hour to 220°C. After keeping warm for 2 hours, the temperature is increased by 12°C per hour to 340°C. After keeping warm for 4 hours, the temperature is increased by 30°C per hour to 600°C. After keeping warm for 2 hours, the temperature is decreased by 240°C per hour to room temperature.
[0019] Furthermore, the transition metal ion solution in S5 is inorganic Cr 3+ Solution or inorganic Co 2+ Solution.
[0020] Further, the inorganic Cr in S5 3+ The concentration of the solution is 0.0015-0.0025 mol / L, and the inorganic Co 2+ The concentration of the solution is 0.005~0.015mol / L.
[0021] Furthermore, the ion doping time in S5 is 2 hours.
[0022] Furthermore, the sintering conditions in S6 are: sintering at 800° C. for 2 hours and sintering at 1280° C. for 2 hours.
[0023] The present invention also provides a colored fused quartz glass doped with transition metal ions, wherein the colored fused quartz glass is prepared by the method described in any one of the above technical solutions.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention proposes a colored fused quartz glass doped with transition metal ions and a preparation method thereof. By reasonably doping transition metal elements and performing heat treatment at a specific temperature and time, a colored glass capable of filtering visible light of a specific wavelength is prepared. Experiments have shown that the glass obtained by the present invention has good light transmittance, an elastic modulus of 68.38 GPa, a hardness of 8.38 GPa, a relative density of more than 99%, and maintains an amorphous state without precipitation of SiO2 crystals.
[0026] The method of the present invention not only has the advantages of short preparation cycle, high product precision, good surface quality, etc., but also can adjust the absorption capacity of glass to light of different wavelengths by doping transition metal ions of different concentrations and types; further control the optical properties of glass, and expand its application in the fields of optical devices. 3+ Fused quartz glass is green and has a strong absorption capacity for blue light with a wavelength range of 435-492nm and red light between 622-760nm. 2+Fused quartz glass is blue and has a strong absorption capacity for yellow light in the wavelength range of 577-597nm and red light in the wavelength range of 622-760nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a colored fused quartz glass sample in an embodiment of the present invention, wherein a is a glass embryo printed by an LCD 3D printer; b is a degreased part; and c is a finished product;
[0028] Figure 2 : is a temperature diagram of the degreasing process in an embodiment of the present invention; wherein a is a temperature diagram during the degreasing process; b is a thermogravimetric and differential scanning calorimetry measurement curve (TG / DSC) of a glass embryo;
[0029] Figure 3 is a temperature diagram during the sintering process in an embodiment of the present invention;
[0030] Figure 4 is a porosity diagram of a degreased part in an embodiment of the present invention;
[0031] Figure 5 is a measurement diagram of characteristic length expansion of a printed part in an embodiment of the present invention;
[0032] Figure 6 is a transmittance diagram of fused silica glass in an embodiment of the present invention;
[0033] Figure 7 is the absorption spectrum of the colored glass in the embodiment of the present invention; wherein Figure a is the absorption spectrum of the colored glass doped with Cr 3+ Absorption spectrum of fused silica glass, Figure b is Co-doped 2+ Absorption spectrum of fused silica glass;
[0034] Figure 8 The XRD patterns of the printed fused quartz glass and KN7980 glass in the embodiments of the present invention are shown in FIG.
[0035] Fig. 9 The XPS spectra of printed fused quartz glass and KN7980 glass in the embodiment of the present invention are shown;
[0036] Fig.10 These are sintered samples under different maximum sintering and heat preservation temperature conditions in the embodiments of the present invention. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, exemplary implementations or embodiments of the present invention will be described below in conjunction with the accompanying drawings. Obviously, the described implementations or embodiments are only implementations or embodiments of a part of the present invention, not all of them. Based on the implementations or embodiments of the present invention, all other implementations or embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present invention.
[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0039] Example 1
[0040] S1. Preparation of photosensitive monomer: 60.8 g of hydroxyethyl acrylate (HEMA), 8.3 g of monomer triethylene glycol diacrylate (TEGDA) and 30.9 g of phenoxyethanol (POE) were weighed and mixed evenly, and then stirred at a speed of 200 rpm for 5 min to obtain a photosensitive monomer;
[0041] S2. Add 0.2 g of diethyl phthalate (DEP), 0.5 g of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO) and 0.05 g of Sudan Orange G to the photosensitive monomer, and stir at a rotation speed of 200 rpm for 5 min to obtain a photosensitive resin.
[0042] Example 2
[0043] S1. Weigh 94g of photosensitive resin and 106g of SiO2 powder, take out 20% of the photosensitive resin for later use, disperse the SiO2 powder in the photosensitive resin of Example 1 in small amounts and multiple times, adjust the rotation speed according to the slurry state during the process to ensure that the stirring process can continue, and after all the SiO2 powder is added, add the taken out 20% of the photosensitive resin into the slurry, and stir at high speed for 10 minutes to dilute the photosensitive slurry.
[0044] S2. Use a vacuum stirrer to further stir to remove bubbles in the slurry, and stir at a speed of 400 rpm for 20 minutes to obtain a bubble-free homogeneous slurry.
[0045] S3, pour the photosensitive slurry into the LCD 3D printer, and set the printing parameters as follows: the excitation light wavelength is 405nm, the average light power density is 5mW / cm 2The printing layer thickness is 0.05mm, and the bottom-up printing method is adopted. When each layer is cured, the printing platform will move up and then drop to the distance of a single printing layer thickness from the bottom of the resin tank. The latest layer of the printed part will be covered with slurry under the dual effects of gravity and air pressure. After printing, the printed part follows the printing platform to separate from the slurry, and the surface slurry is removed to obtain the following Figure 1 The three-dimensional glass embryo shown in a.
[0046] S4. Place the glass embryo in a tube furnace and raise the temperature from 25°C to 800°C at 5°C / min in an air atmosphere to obtain the following Figure 2 The TG / DSC curve shown in b roughly divides the organic matter removed from the print into four categories according to the four turning points in the weight loss process.
[0047] The DSC curve obtained in this embodiment is used to infer the changes in the thermodynamic properties of the printed part during the heating process to further determine the chemical change process of the organic matter and the temperature at which the organic matter decomposes and volatilizes.
[0048] Example 3
[0049] S1. Put the glass embryo obtained in Example 2 into a tube furnace and heat it in an air atmosphere by programmed heating. Figure 2 As shown in a, the temperature is raised to 220°C at 24°C per hour. After 2 hours of heat preservation, the temperature is raised to 340°C at 12°C per hour. After 4 hours of heat preservation, the temperature is further raised to 600°C at 30°C per hour. After 2 hours of heat preservation, the temperature is further lowered to room temperature at 240°C per hour. The result is as follows Figure 1 b shows the degreased parts.
[0050] S2. Conduct thermal expansion test on degreased parts, such as Figure 5 As shown, the volume change of the sample is very small during the organic matter removal process, and the quality of the sample tends to be stable in the range of 1240℃ ~ 1320℃ during thermal expansion.
[0051] The degreasing process of this embodiment is carried out in a tube furnace. The oxygen in the furnace decomposes the polymer binder in the glass embryo, so that the degreased part has many pores and is white in color. The porosity of the degreased part is as follows: Figure 4 As shown; the existence of these pores allows the transition metal ion solution to penetrate, which is beneficial to the doping of metal ions. Figure 2
[0052] Example 4
[0053] The degreased parts obtained in Example 3 were placed in a tube furnace and sintered under air atmosphere at a temperature as Figure 3As shown, the temperature is increased from 180°C per hour to 800°C, and after being kept warm for two hours, the temperature is increased from 120°C per hour to 1280°C, and after being kept warm for two hours, the temperature is further decreased from 240°C per hour to room temperature to obtain fused quartz glass.
[0054] The transmittance of the fused silica glass of this embodiment and the commercial KN7980 glass was tested, and the results are as follows: Figure 6 As shown, the transmittance of the fused silica glass of this embodiment is greater than 90% in the wavelength range of 360-900nm, and still has a transmittance of more than 75% at a wavelength of 250nm, which is basically consistent with the ultraviolet-visible light transmittance spectrum of commercial KN7980 glass; the elastic modulus of the fused silica glass of this embodiment is 68.38GPa, the hardness is 8.38GPa, and the relative density is greater than 99% of the fused silica glass.
[0055] XRD tests were performed on the fused silica glass of this embodiment and the commercial KN7980 glass. The results are as follows: Figure 8 As shown in the figure, compared with the KN7980 glass, it can be seen that the fused silica glass of this embodiment does not have a sharp strong diffraction peak in the entire spectrum, and no crystalline phase (such as cristobalite) is detected, while there is also an obvious broad diffraction peak at 2θ=22.5°, which is attributed to the broad diffraction peak of SiO2, indicating that SiO2 in the fused silica glass finally obtained by sintering exists in an amorphous form and remains in an amorphous state, without precipitation of SiO2 crystals.
[0056] XPS spectrum test was performed on the fused silica glass and KN7980 glass of this embodiment to further analyze and determine the element composition and valence state of the fused silica glass. The results are as follows: Fig. 9 As shown, the results show that there is almost no difference in element composition and valence state between the fused silica glass of this embodiment and the KN7980 glass.
[0057] Comparative Example 1
[0058] Fused quartz glass was prepared according to the method of Example 4, except that the maximum sintering temperature during the sintering process was 1240°C.
[0059] Comparative Example 2
[0060] Fused quartz glass was prepared according to the method of Example 4, except that the maximum sintering temperature during the sintering process was 1260°C.
[0061] Comparative Example 3
[0062] Fused quartz glass was prepared according to the method of Example 4, except that the maximum sintering temperature during the sintering process was 1300°C.
[0063] Comparative Example 4
[0064] Fused quartz glass was prepared according to the method of Example 4, except that the maximum sintering temperature during the sintering process was 1320°C.
[0065] like Fig.10 As shown, by comparing the glass samples under different maximum sintering temperature conditions, the glass sample at 1240°C is not completely dense, the glass sample at 1320°C has crystals precipitated, and the transparency of the glass samples at 1260°C and 1300°C is worse than that at 1280°C.
[0066] Example 5
[0067] S1. Weigh Cr(NO3)3·9H2O powder and prepare 0.0015 mol / L transition metal ion Cr 3+ of ethanol solution.
[0068] S2, immersing the degreased part of Example 3 in a transition metal ion Cr 3+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0069] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 1.23 μmol / cm 3 Cr 3+ Tinted glass.
[0070] In this embodiment, the doping concentration of transition metal ions in the fused silica glass is calculated based on the porosity, that is:
[0071] cg=cs P ρg
[0072] Where c g ——ion doping concentration in glass (mol / L);
[0073] c s ——ion doping concentration in the solution (mol / L);
[0074] P——Porosity of degreased parts (cm 3 / g / );
[0075] ρ g ——Density of fused quartz glass (g / cm 3 ).
[0076] Example 6
[0077] S1. Weigh Cr(NO3)3·9H2O powder and prepare 0.002 mol / L transition metal ion Cr 3+ of ethanol solution.
[0078] S2, immersing the degreased part of Example 3 in a transition metal ion Cr 3+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0079] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 1.63 μmol / cm 3 Cr 3+ Tinted glass.
[0080] Example 7
[0081] S1. Weigh Cr(NO3)3·9H2O powder and prepare 0.0025 mol / L transition metal ion Cr 3+ of ethanol solution.
[0082] S2, immersing the degreased part of Example 3 in a transition metal ion Cr 3+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0083] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 2.04 μmol / cm 3 Cr 3+ Tinted glass.
[0084] Example 8
[0085] S1. Weigh Co(NO3)2·6H2O powder and prepare 0.005 mol / L transition metal ion Co 2+ of ethanol solution.
[0086] S2, immersing the degreased part of Example 3 in a transition metal ion Co 2+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0087] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 4.08 μmol / cm 3 Co 2+ Tinted glass.
[0088] Example 9
[0089] S1. Weigh Co(NO3)2·6H2O powder and prepare 0.010 mol / L transition metal ion Co 2+ of ethanol solution.
[0090] S2, immersing the degreased part of Example 3 in a transition metal ion Co 2+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0091] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 8.17 μmol / cm 3 Co 2+ Tinted glass.
[0092] Example 10
[0093] S1. Weigh Co(NO3)2·6H2O powder and prepare 0.015 mol / L transition metal ion Co 2+ of ethanol solution.
[0094] S2, immersing the degreased part of Example 3 in a transition metal ion Co 2+ The sample was immersed in the solution for 2 hours. After immersion, it was taken out with tweezers and placed in a drying oven at 50°C for 1 hour.
[0095] S3, put the dried degreased parts into a tube furnace, and raise the temperature from 180°C per hour to 800°C in air atmosphere. After keeping the temperature for two hours, the temperature is raised from 120°C per hour to 1280°C. After keeping the temperature for two hours, the temperature is lowered from 240°C per hour to room temperature. The obtained product contains 12.25 μmol / cm 3 Co 2+ Tinted glass.
[0096] Cr-doped samples of Examples 5 to 7 3+ The fused silica glass is green. 3+Colored glass is tested by infrared absorption spectrum, and the results are as follows Figure 7 As shown in a, it has strong absorption ability in the wavelength range of 435-492nm cyan light and 622-760nm red light;
[0097] Co-doped Examples 8 to 10 2+ The fused silica glass exhibits a blue color. 2+ Colored glass is tested by infrared absorption spectrum, and the results are as follows Figure 7 As shown in b, it has a strong absorption ability for yellow light in the wavelength range of 577-597nm and red light in the wavelength range of 622-760nm.
[0098] The principle of the present invention is:
[0099] In the photosensitive monomer of the present invention, HEMA molecules contain C=C, and can undergo polymerization reaction to generate macromolecules under the induction of a photoinitiator. The hydroxyl group at the end of the molecule can form a hydrogen bond with the silanol group on the surface of SiO2, forming a solvation layer around the SiO2 powder, and accommodating a large amount of nano-SiO2 powder without adding a dispersant; TEGDA has low viscosity, good solubility and high polarity, and two C=C double bonds exist in the molecule, so the photocuring rate is fast, which is conducive to the photocuring process; POE also has a hydroxyl group at the end of the molecule, which is conducive to the dispersion of SiO2 powder, but its properties are uncertain, and it does not participate in the reaction during the photocuring molding process, and is removed in the degreasing process. The generated pores are conducive to the removal of other organic matter, and the purity of the fused quartz glass can be indirectly improved.
[0100] In the photosensitive resin, TPO is a photoinitiator with an obvious light absorption peak at around 405nm. When excited by ultraviolet rays, it will produce free radicals that cause a chain polymerization reaction in the slurry. Sudan Orange G, as an ultraviolet absorber, can inhibit lateral photopolymerization at a wavelength of 405nm, control the curing depth, and improve printing accuracy by reducing the xy dimensional deviation caused by light scattering and z-axis over-curing. DEP is a plasticizer that has a weak effect on the viscosity of the slurry, but can increase the strength of the photopolymerization product and reduce the cracking of the printed parts.
[0101] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing colored fused quartz glass doped with transition metal ions, characterized in that: The steps include: S1, prepare photosensitive resin, disperse SiO2 powder in the photosensitive resin to obtain photosensitive slurry; S2, using light-curing technology to print the photosensitive slurry to form a three-dimensional glass embryo; S3, performing thermogravimetric and differential scanning calorimetry tests on the glass embryo, and constructing thermogravimetric and differential scanning calorimetry data curves during the construction process; S4, determining the degreasing conditions according to the thermogravimetric and differential scanning calorimetry data curves, and performing degreasing heat treatment on the glass embryo; S5, placing the degreased parts in a transition metal ion solution for ion doping, and drying; S6. Perform a thermal expansion test on the degreased part after doping to determine the sintering conditions, and perform a sintering treatment on the degreased part after doping to obtain the colored glass doped with transition metal ions.
2. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 1, characterized in that: The mass ratio of the photosensitive resin to SiO2 in S1 is 47:
53.
3. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 1, characterized in that: The photosensitive resin in S1 includes, by mass, 100 parts of a photosensitive monomer, 0.2 parts of diethyl phthalate, 0.5 parts of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and 0.05 parts of Sudan Orange G; The photosensitive monomers include, by mass, 60.8 parts of hydroxyethyl acrylate, 8.3 parts of monomer triethylene glycol diacrylate and 30.9 parts of phenoxyethanol.
4. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 1, characterized in that: The degreasing conditions in S4 are: heating at 220° C. for 2 hours, 340° C. for 4 hours and 600° C. for 2 hours in an air atmosphere by a programmed temperature increase method.
5. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 4, characterized in that: The specific process of the degreasing heat treatment described in S4 is: using a programmed temperature rising method in an air atmosphere, the temperature is raised from 24°C per hour to 220°C, after keeping warm for 2 hours, the temperature is raised from 12°C per hour to 340°C, after keeping warm for 4 hours, the temperature is further raised from 30°C per hour to 600°C, after keeping warm for 2 hours, the temperature is then dropped from 240°C per hour to room temperature.
6. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 1, characterized in that: The transition metal ion solution in S5 is inorganic Cr 3+ Solution or inorganic Co 2+ Solution.
7. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 6, characterized in that: Inorganic Cr 3+ The concentration of the solution is 0.0015-0.0025 mol / L, and the inorganic Co 2+ The concentration of the solution is 0.005~0.015mol / L.
8. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 7, characterized in that: The ion doping time in S5 is 2 h.
9. The method for preparing colored fused quartz glass doped with transition metal ions according to claim 1, characterized in that: The sintering conditions in S6 are: sintering at 800° C. for 2 hours and sintering at 1280° C. for 2 hours.
10. A colored fused quartz glass doped with transition metal ions, characterized in that: The colored fused quartz glass is prepared by the method described in any one of claims 1 to 9 above.