Preparation method of sapphire optical fiber high-temperature-resistant cladding desensitized by intrinsic temperature
By preparing negative expansion cladding on the surface of sapphire optical fiber, the high-order mode and temperature crosstalk problems are solved using β-lithium cylindrical and ultraviolet curing technology, mode suppression and temperature desensitization are achieved, and the measurement accuracy and high-temperature resistance of the sensor are improved. .
Patent Information
- Application Number
- CN202410970028.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Commercial sapphire fibers have advanced modes and temperature crosstalk problems, resulting in difficulty in demodulation of signals and reduced measurement accuracy. Existing solutions such as the use of reference fiber sensors have system errors.
A high-temperature resistant cladding was prepared on the surface of sapphire optical fiber using negative expansion material β-lithium cylindrical and ultraviolet curing technology. A cladding with pattern suppression and temperature desensitization characteristics were prepared by mixing ultraviolet-sensitive resin liquid for ultraviolet curing and high-temperature sintering.
Effectively suppresses higher-order modes, reduces temperature sensitivity, improves sensor demodulation accuracy, simplifies process flow, and reduces costs. It is suitable for sapphire fiber sensors of different structures.
Smart Images

Figure CN118908593A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of optical fiber sensing, and in particular relates to a method for preparing a high temperature resistant cladding of an intrinsic temperature desensitized sapphire optical fiber. Background Art
[0002] Sapphire optical fiber has excellent light transmission performance in the ultraviolet to mid-infrared band, a melting point above 2000°C, and a high laser damage threshold. It is an ideal high-temperature resistant waveguide and is widely used in the field of high-temperature sensing. At present, commercial sapphire optical fiber is grown and prepared by the pulling method, guided mode method, laser heating base method, etc. The single crystal growth rate is fast, the cycle is short, and the size is controllable (Wang D, Hou W, Na LI, et al. Defects and Optical Property of Single-crystal Sapphire Fibers Grown by Edge-defined Film-fed Growth Method [J]. Journal of Inorganic Materials, 2020, 35 (9): 573). However, current commercial sapphire optical fibers face two disadvantages: First, there are a large number of high-order modes, which is not conducive to signal reception and demodulation; second, there is temperature crosstalk, which is not conducive to high-precision measurement of a single parameter (ABW, AY N, AXQ, et al. Review of High Temperature Measurement Technology Based on Sapphire Optical Fiber[J]. Measurement, 2021, 184:1009868).
[0003] Unlike common quartz optical fibers, commercial sapphire optical fibers are single crystals with no cladding structure on the outer surface. Therefore, the transmitted light cannot be effectively bound in the optical fiber, and it is easy to excite high-order modes, which makes it difficult for sapphire optical fiber sensors to distinguish the measured signals, difficult to demodulate the signals, and greatly reduce the measurement accuracy. In recent years, researchers have prepared cladding structures on the surface of sapphire optical fibers through magnetron sputtering, vapor deposition, solution corrosion, chemical treatment, etc., which effectively suppress high-order modes and reduce the transmission loss of sapphire optical fibers (Chen H, Buric M, Ohodnicki PR, et al. Review and perspective: Sapphire optical fiber cladding development for harsh environment sensing [J]. Applied Physics Reviews, 2018, 5 (1): 011102). However, the sapphire optical fiber cladding reported so far often has many problems such as complex preparation process, high processing cost, and high temperature intolerance. In addition, the additional cladding structures reported cannot reduce the temperature drift of the sensor. Due to the thermo-optical coefficient of sapphire optical fiber (12.6×10 -6 / ℃) and thermal expansion coefficient (5×10 -6 / ℃) are both high, so in actual use, the sensor inevitably has the problem of temperature crosstalk, that is, the physical quantity to be measured and the ambient temperature are cross-sensitive. Especially in the detection of quasi-static signals, the signal response caused by temperature disturbance is not easy to filter out, which makes it difficult to distinguish and identify the physical quantity to be measured, and it is difficult to achieve high-precision measurement of a single parameter. At present, the usual solution to the temperature crosstalk problem of sapphire fiber optic sensors is to use a reference fiber optic sensor that is only sensitive to temperature to test in the same environment, so as to eliminate the temperature influence and achieve temperature compensation. This method is simple, convenient and widely used, but in actual working conditions, heat is transferred in a non-single path, and there are differences in the temperature field distribution between the experimental sensor and the reference sensor, which will cause system errors. Considering the requirements of measurement accuracy, sensitivity, simplicity, integration and other aspects, the research on the temperature cross-sensitivity problem of sapphire fiber optic sensors should consider the transition from non-intrinsic compensation to intrinsic compensation. Summary of the invention
[0004] If the additional cladding structure can effectively suppress temperature crosstalk and reduce the fiber mode at the same time, it will achieve the effect of killing two birds with one stone.
[0005] In view of the current problems of complex sapphire optical fiber modes and temperature crosstalk in the sensing process, the present invention proposes a method for preparing a sapphire optical fiber cladding that has mode suppression and temperature desensitization characteristics and is resistant to high temperatures based on negative expansion materials and ultraviolet curing technology.
[0006] The present invention reduces the transmission mode of sapphire optical fiber by preparing a high temperature resistant negative expansion cladding on the outer surface of sapphire optical fiber, and at the same time has the effect of temperature desensitization. The present invention adopts β-eucryptite negative expansion material and ultraviolet curing molding technology to realize the controllable preparation of sapphire optical fiber cladding, simplify the process flow, reduce the preparation cost, shorten the processing cycle, and is suitable for sapphire optical fiber sensors with different structures.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] The object of the present invention is to provide a method for preparing a high temperature resistant cladding of a sapphire optical fiber with intrinsic temperature desensitization, comprising the following steps:
[0009] Step 1, mixing an ultraviolet absorber, a photosensitizer, an inhibitor, a crosslinking agent and negative expansion material β-eucryptite nanoparticles, and fully stirring to obtain an ultraviolet sensitive resin liquid;
[0010] Step 2, cleaning the sapphire optical fiber, and then placing it on a polytetrafluoroethylene capillary, filling it with UV-sensitive resin liquid, sealing it, and curing it with UV light. After curing, the capillary is peeled off;
[0011] Step 3, then degrease in stages;
[0012] Step 4: Then sinter at high temperature to obtain the cladding on the surface of the sapphire optical fiber.
[0013] It is further defined that the ultraviolet absorber is hydroquinone.
[0014] It is further defined that the photosensitizer is 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0015] It is further defined that the inhibitor is 2-hydroxyethyl methacrylate and 2-phenoxyethanol.
[0016] It is further defined that the crosslinking agent is 2-phenoxyethanol tetra(ethylene glycol) diacrylate.
[0017] It is further defined that the volume ratio of the ultraviolet absorber, the photosensitizer, the inhibitor and the cross-linking agent is 2:1:3:4.
[0018] It is further defined that in the ultraviolet sensitive resin solution, the molar concentration of the β-eucryptite is 20%-40%, and the particle size is 50nm-200nm.
[0019] Further defined, UV curing under 385nm light.
[0020] It is further defined that the diameter of the polytetrafluoroethylene capillary is 100 μm-500 μm.
[0021] It is further defined that the distance between the UV light source and the sapphire optical fiber is 20cm-60cm, and the light intensity is 100mW / cm 2
[0022] It is further defined that the staged degreasing process is as follows: first, increase the temperature from room temperature to 150°C within 10 minutes, and keep it warm for 30 minutes; then increase the temperature to 325°C within 20 minutes, and keep it warm for 30 minutes; then increase the temperature to 375°C within 10 minutes, and keep it warm for 30 minutes; then increase the temperature to 450°C within 15 minutes, and keep it warm for 30 minutes; then increase the temperature to 600°C within 15 minutes, and keep it warm for 120 minutes; then naturally cool to room temperature.
[0023] It is further defined that the high temperature sintering process is as follows: first, increase the temperature from room temperature to 800°C within 120 minutes, and keep it warm for 60 minutes; then increase the temperature to 1200°C within 120 minutes, and keep it warm for 60 minutes; then increase the temperature to 1300°C within 10 minutes, and keep it warm for 60 minutes; ④ naturally cool to room temperature.
[0024] A cladding obtained by any of the methods described above.
[0025] The present invention can determine that the negative expansion cladding effectively suppresses high-order modes and reduces the number of fiber modes through fiber mode field distribution observation, mode field radius measurement and optical simulation. At the same time, by writing gratings on sapphire optical fibers or preparing FP cavity sensors, it can be determined that the negative expansion cladding reduces the temperature crosstalk of sapphire optical fibers and improves the measurement accuracy.
[0026] The present invention prepares a negative expansion cladding on the surface of sapphire optical fiber through material and structural design combined with ultraviolet curing rapid prototyping process. The method of the present invention can effectively suppress the high-order mode of sapphire optical fiber, reduce temperature sensitivity, and avoid high-temperature damage to the optical fiber, thereby improving the demodulation accuracy of the sensor and reducing transmission light loss. The present invention has a simple structure, low cost, time-saving and high efficiency, and can be applied to grating, Fabry-Perot, Michelson, Mach-Zehnder and other sapphire optical fiber high-temperature sensors.
[0027] The preparation method of the present invention can suppress the excitation of high-order modes of sapphire optical fibers and intrinsically reduce the temperature sensitivity of optical fibers, thereby effectively improving the accuracy of sensors.
[0028] The present invention adopts ultraviolet curing technology to achieve controllable preparation of sapphire optical fiber cladding, avoids cumbersome process flow, shortens processing cycle, and greatly reduces cost.
[0029] Based on the excellent characteristics of mode suppression, temperature desensitization, high temperature tolerance, etc., the sapphire optical fiber negative expansion cladding can be flexibly applied to high-temperature sensing devices of different structures.
[0030] In order to further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the attached drawings are only provided for reference and illustration and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the sapphire optical fiber and cladding structure of the present invention;
[0032] Figure 2 The mode field after the cladding of the sapphire optical fiber is added according to the method of the present invention;
[0033] Figure 3 This is a simulation diagram of sapphire optical fiber mode number-cladding refractive index-core diameter size according to the method of the present invention. DETAILED DESCRIPTION
[0034] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, and do not limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0035] Embodiment 1: The method for preparing a high temperature resistant cladding of a sapphire optical fiber with intrinsic temperature desensitization in this embodiment is achieved by the following steps:
[0036] Step 1, mixing an ultraviolet absorber, a photosensitizer, an inhibitor, a crosslinking agent and negative expansion material β-eucryptite nanoparticles, and fully stirring (stirring rate 600r / min) to obtain an ultraviolet sensitive resin liquid;
[0037] The ultraviolet absorber is hydroquinone, the photosensitizer is 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, the inhibitor is 2-hydroxyethyl methacrylate and 2-phenoxyethanol, the crosslinking agent is 2-phenoxyethanol tetra(ethylene glycol) diacrylate, the average particle size of the negative expansion material β-eucryptite nanoparticles is 270nm, the volume ratios of the photosensitizer, the inhibitor and the crosslinking agent are 2:1:3:4 respectively, and the molar concentration of the β-eucryptite is 30%.
[0038] Step 2: Clean the sapphire optical fiber using a standard cleaning process, then place it on a polytetrafluoroethylene capillary, fill it with UV-sensitive resin liquid, seal it, and cure it under UV light at 385nm. After curing, peel off the capillary;
[0039] The diameter of the polytetrafluoroethylene capillary is 10μm, 20μm or 37.5μm. The distance between the ultraviolet light source and the sapphire optical fiber is 30cm, and the light intensity is 100mW / cm 2; The standard cleaning process is to wipe lightly with alcohol to remove dust.
[0040] Step 3, then degrease in stages; specifically: ① Raise the temperature from room temperature to 150°C within 10 minutes, and keep warm for 30 minutes; ② Raise the temperature to 325°C within 20 minutes, and keep warm for 30 minutes; ③ Raise the temperature to 375°C within 10 minutes, and keep warm for 30 minutes; ④ Raise the temperature to 450°C within 15 minutes, and keep warm for 30 minutes; ⑤ Raise the temperature to 600°C within 15 minutes, and keep warm for 120 minutes; ⑥ Cool naturally to room temperature.
[0041] Step 4: Then sintering at high temperature to obtain the cladding on the surface of the sapphire optical fiber;
[0042] In step 4, the high temperature sintering procedure is as follows: ① from room temperature to 800°C within 120 minutes, and keep warm for 60 minutes; ② from room temperature to 1200°C within 120 minutes, and keep warm for 60 minutes; ③ from room temperature to 1300°C within 10 minutes, and keep warm for 60 minutes; ④ naturally cool to room temperature.
[0043] In this embodiment, Figure 3 As shown by Figure 3 It can be seen that the sapphire optical fiber cladding of the present invention can be prepared through the steps of preparing a UV-sensitive resin liquid, UV curing, degreasing, sintering, etc.
[0044] The above describes the specific embodiments of the present invention. It should be noted that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various modifications or variations within the scope of the claims, which does not affect the essential content of the present invention.
Claims
1. A method for preparing a high temperature resistant cladding of an intrinsic temperature desensitized sapphire optical fiber, characterized in that: The following steps are involved: Step 1, mixing an ultraviolet absorber, a photosensitizer, an inhibitor, a crosslinking agent and negative expansion material β-eucryptite nanoparticles, and fully stirring to obtain an ultraviolet sensitive resin liquid; Step 2, cleaning the sapphire optical fiber, and then placing it on a polytetrafluoroethylene capillary, filling it with UV-sensitive resin liquid, sealing it, and curing it with UV light. After curing, the capillary is peeled off; Step 3, then degrease in stages; Step 4: Then sinter at high temperature to obtain the cladding on the surface of the sapphire optical fiber.
2. The method according to claim 1, characterized in that: The ultraviolet absorber is hydroquinone; the photosensitizer is 2,4,6-trimethylbenzoyldiphenylphosphine oxide; the inhibitor is 2-hydroxyethyl methacrylate and 2-phenoxyethanol; and the crosslinking agent is 2-phenoxyethanol tetra(ethylene glycol) diacrylate.
3. The method according to claim 1, characterized in that: The volume ratio of the ultraviolet absorber, the photosensitizer, the inhibitor and the cross-linking agent is 2:1:3:
4.
4. The method according to claim 1, characterized in that: In the ultraviolet sensitive resin solution, the molar concentration of the beta-eucryptite is 20%-40%, and the particle size is 50nm-200nm.
5. The method according to claim 1, characterized in that: UV curing under 385nm light.
6. The method according to claim 1, characterized in that: The diameter of the polytetrafluoroethylene capillary is 100 μm-500 μm.
7. The method according to claim 1, characterized in that: The distance between the UV light source and the sapphire optical fiber is 20cm-60cm, and the light intensity is 100mW / cm 2 .
8. The method according to claim 1, characterized in that: The staged degreasing process is as follows: first, raise the temperature from room temperature to 150°C within 10 minutes, and keep it warm for 30 minutes; then raise the temperature to 325°C within 20 minutes, and keep it warm for 30 minutes; then raise the temperature to 375°C within 10 minutes, and keep it warm for 30 minutes; then raise the temperature to 450°C within 15 minutes, and keep it warm for 30 minutes; then raise the temperature to 600°C within 15 minutes, and keep it warm for 120 minutes; then naturally cool to room temperature.
9. The method according to claim 1, characterized in that: The high-temperature sintering process is as follows: first, increase the temperature from room temperature to 800°C within 120 minutes, and keep it warm for 60 minutes; then increase the temperature to 1200°C within 120 minutes, and keep it warm for 60 minutes; then increase the temperature to 1300°C within 10 minutes, and keep it warm for 60 minutes; ④ naturally cool to room temperature.
10. A cladding obtained by the method according to any one of claims 1 to 9.