Artificial aggregate and preparation method thereof

Through the design of artificial aggregates, the mixing of metal shells and porous structural ceramics with B4C or Gd2O3 is solved, and the existing serpentine concrete is high cost and poor working performance is achieved, and high moisture content and excellent neutron shielding ability are achieved. Meet the large-scale application needs of nuclear facilities.

CN118908605AActive Publication Date: 2024-11-08SHANGHAI CONSTRUCTION GROUP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411037240.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The application of existing serpentine concrete in nuclear facilities has problems such as high production costs, poor working performance and difficult to improve moisture content, which cannot meet the needs of large-scale applications.

Method used

Using artificial aggregates, including metal shells and porous structure ceramic raw materials mixed with B4C or Gd2O3, a high moisture content concrete is formed by firing and post-treatment. The metal shell is used to accommodate porous structures and provide support, and water-based liquid is used for Slow down fast neutrons.

Benefits of technology

It has achieved high moisture content, excellent neutron shielding ability and thermal neutron absorption capacity, meeting the needs of neutron shielding structures in nuclear facilities, and the production process is simple and industrialized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908605A_ABST
    Figure CN118908605A_ABST
Patent Text Reader

Abstract

The invention relates to an artificial aggregate and a preparation method thereof, and belongs to the technical field of preparation of anti-radiation concrete raw materials. The artificial aggregate comprises a metal shell, a porous structure and water-based liquid, and the metal shell is of a sealed structure and used for containing the porous structure; the porous structure is formed by mixing ceramsite raw materials and powdery B4C or Gd2O3 with the weight ratio of 1%-10%, the weight of the B4C accounts for 20%-80% of the total weight of the powdery B4C or Gd2O3, the particle size of the powdery B4C or Gd2O3 is 10 micrometers, the powdery B4C or Gd2O3 is formed into a specified shape, and an obtained formed body is dried and fired. The water-based liquid is natural water, tap water or boric acid solution contained in pores of the porous structure. The artificial aggregate is convenient to obtain, the preparation process is simple, the production process is highly industrialized, novel concrete with the water content, workability, fast neutron moderation capacity and thermal neutron absorption capacity superior to those of existing concrete can be prepared, and the requirements of nuclear radiation in special nuclear facilities, especially neutron shielding structure construction are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of raw materials for radiation-proof concrete, and in particular relates to an artificial aggregate and a preparation method thereof. Background Art

[0002] In the construction of nuclear power plants and other facilities, concrete structures are an important part of the radiation shielding layer. Water is the best moderator for fast neutrons produced by nuclear reactions. Using serpentine (a mineral containing about 13% by weight of bound water) as a concrete aggregate in concrete materials can play a good neutron shielding role and has been used in a few nuclear facilities.

[0003] However, as a natural ore, serpentine aggregate has many impurities and high production costs. The resulting serpentine concrete has poor workability and its moisture content is difficult to further increase, which cannot meet the needs of large-scale applications in nuclear facilities.

[0004] Therefore, there is an urgent need to provide an artificial aggregate and a preparation method thereof to meet the needs of large-scale application in nuclear facilities. Summary of the invention

[0005] The invention provides an artificial aggregate and a preparation method thereof, which can realize large-scale production and is particularly suitable for the preparation of high-water-content concrete.

[0006] In order to solve the above technical problems, the present invention includes the following technical solutions:

[0007] An artificial aggregate, comprising:

[0008] A metal shell, wherein the metal shell is a sealed structure and is used to accommodate the porous structure;

[0009] A porous structure, wherein the porous structure is formed into a predetermined shape by mixing ceramsite raw materials with 1% to 10% by weight of powdered B4C or Gd2O3, wherein the weight of B4C accounts for 20% to 80% of the total weight of the powder, and the particle size of the powder is about 10 microns, and the formed body is dried and then fired; and

[0010] The water-based liquid is natural water, tap water or boric acid solution contained in the pores of the porous structure.

[0011] Furthermore, the porosity of the porous structure is greater than 30%, and the cylinder pressure strength is greater than 10 MPa.

[0012] Furthermore, the ceramsite is at least one selected from aluminum oxide particles, silicon oxide particles, silicon carbide particles and silicon nitride particles.

[0013] Furthermore, the metal shell is a metal spherical shell or other hollow special-shaped closed structure, and the metal is made of stainless steel.

[0014] Furthermore, the outer radius of the metal spherical shell is R, and the thickness is t, wherein the value range of R is 1.5 mm to 20 mm, then Where, α is the safety factor, which ranges from 1.5 to 2.0; p = 1.55 MPa is the critical boiling pressure of water at 200 °C; σ y =360MPa is the yield stress of the metal material. This condition is based on the formula of film stress generated by internal pressure of a spherical shell in theoretical mechanics, and the film stress must be less than the yield stress of the metal spherical shell material. Obtained by conversion.

[0015] The present invention also provides a method for preparing an artificial aggregate, the method comprising the following steps:

[0016] Step S1: using natural clay, blast furnace slag powder and other industrial solid wastes, engineering waste soil as basic raw materials, adding 1% to 10% by weight of powdered B4C or Gd2O3, adding water and a foaming agent to mix, and making spherical particles, the specific mass ratio is as follows;

[0017]

[0018] The firing temperature was controlled at 1300°C for 3 h;

[0019] The particles are expanded by a foaming agent and fired to release the internal moisture to obtain porous ceramsite. Finally, the obtained ceramsite is screened and classified according to its size, cylinder pressure strength and porosity.

[0020] Step S2: soaking the ceramsite prepared in step S1 in water to absorb the liquid until saturated;

[0021] Step S3: grouping the ceramsite soaked in step S2 according to their sizes, and placing the grouped ceramsite into a freezer to freeze the outer layer of liquid and lock the inner liquid;

[0022] Step S4: placing the ceramsite frozen in step S3 in a high temperature resistant scooping net, immersing it in the molten metal, and scooping it out after the surface is covered with a layer of metal shell to obtain liquid-coated particles;

[0023] Step S5: post-processing the liquid-coated particles obtained in step S4, cutting and separating the adhered artificial aggregates, reducing the defects of the metal shell by tempering, performing heating tests and pressure tests on the obtained ceramsite, screening and obtaining qualified products, and obtaining artificial aggregates.

[0024] Furthermore, the step S3 comprises:

[0025] The size groups are separated according to the radius difference of 0.5 mm; and the average radius R corresponding to each group is determined in advance through experiments. 平均 , which satisfies the freezing time T required for the outer layer of liquid to freeze but the inner liquid to not freeze 冷冻 (R 平均 ) to prevent all liquid from freezing and cracking and destroying the porous structure; the unified freezing time of this group is taken as T 冷冻 (R 平均 ). For example, using a -20°C freezer, R 平均 =10mm group freezing time T 冷冻 0.5h.

[0026] Furthermore, the step S4 comprises:

[0027] According to the different size groups, the average radius R of each group is determined in advance through experiments. 平均 The minimum soaking time T of ceramsite 浸泡 (R 平均 ), ensuring that its surface is covered with a metal shell with a thickness of t; the unified immersion time of this group is taken as T 浸泡 (R 平均 ). For example, in molten steel at 1500℃, R 平均 =10mm grouping, immersion time T 浸泡 is 15s.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] The present invention provides an artificial aggregate, which includes a metal shell, a porous structure and water. The metal shell is a sealing structure for containing the porous structure. The porous structure is formed into a specified shape by mixing ceramsite raw materials with 1% to 10% by weight of powdered B4C or Gd2O3, and then dried and fired to obtain a formed body. The water-based liquid is natural water, tap water or boric acid solution contained in the pores of the porous structure. The artificial aggregate is easy to obtain, has a simple preparation process, and can be highly industrialized. A new type of concrete can be prepared, which is superior to existing concrete in terms of water content, workability, fast neutron moderation ability, and thermal neutron absorption ability, and meets the needs of nuclear radiation in special nuclear facilities, especially the construction of neutron shielding structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of the structure of an artificial aggregate according to an embodiment of the present invention;

[0031] Figure 2 Schematic diagram of the relationship between the thickness of the metal shell and the outer radius of the spherical shell in an artificial aggregate according to an embodiment of the present invention;

[0032] Figure 3It is a flow chart of a method for preparing artificial aggregate according to an embodiment of the present invention.

[0033] In the figure:

[0034] 1-Metal shell, 2-Porous structure, 3-Water-based liquid. DETAILED DESCRIPTION

[0035] The following is a further detailed description of an artificial aggregate and a preparation method thereof provided by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. For the convenience of description, the "upper" and "lower" described below are consistent with the upper and lower directions of the accompanying drawings, but this cannot be a limitation of the technical solution of the present invention.

[0036] Embodiment 1

[0037] Combine the following Figures 1 to 3 , the structural composition of the artificial aggregate of the present invention is described in detail.

[0038] Please continue to refer to Figure 1 and Figure 2 An artificial aggregate includes a metal shell 1, a porous structure 2 and water. The metal shell 1 is a sealed structure for containing the porous structure 2. The porous structure 2 is a mixture of ceramsite raw materials and 1% to 10% by weight of powdered B4C or Gd2O3, wherein the weight of B4C accounts for 20% to 80% of the total weight of the powder, and the particle size of the powder is 10 microns. The powder is formed into a specified shape, and the obtained formed body is dried and fired. The water-based liquid 3 is natural water, tap water or boric acid solution contained in the pores of the porous structure 2. The water-based liquid 3 is the main component for slowing down the fast neutrons generated by nuclear facilities.

[0039] In this embodiment, more preferably, the porosity of the porous structure 2 is greater than 30%, and the cylinder pressure strength is greater than 10MPa. On the one hand, the porous structure supports the spherical shell so that the spherical shell does not undergo plastic deformation or buckling under normal working pressure; on the other hand, the porous structure holds the liquid; finally, the B and Gd elements can effectively absorb neutrons.

[0040] In this embodiment, more preferably, the ceramsite is at least one selected from aluminum oxide particles, silicon oxide particles, silicon carbide particles and silicon nitride particles.

[0041] In this embodiment, more preferably, the metal shell is a metal spherical shell or other hollow special-shaped closed structure, and the metal is made of stainless steel. The metal shell is used to wrap the porous structure 2, so the shape of the metal shell is determined by the formed shape of the porous structure 2, and the formed body of the porous structure 2 can be any structure. Therefore, the shape of the metal shell is not limited here, as long as it can wrap the porous structure 2 and completely seal it.

[0042] In this embodiment, more preferably, the radial stress of the spherical shell satisfies the classical formula in theoretical mechanics:

[0043] The radial stress increases the magnification factor, which is less than the yield stress of the spherical shell, that is,

[0044] Through formula conversion, the thickness of the spherical shell satisfies the following formula:

[0045] In the formula, σ l is the radial stress of the spherical shell. The water-based liquid is water. The maximum operating temperature of the design condition is 200°C. At this temperature, the critical boiling pressure of water is p = 1.55 MPa. For example, a metal spherical shell is selected, and the yield stress σ of the spherical shell is y =360MPa; R is in the range of 1.5mm to 20mm; α is the safety factor, which is 1.5 to 2.0. Taking a particle with an outer radius of R = 10mm as an example, according to the formula The calculated thickness of the spherical shell t is at least 0.0323 mm; if the outer radius of a particle R = 20 mm, the thickness of the spherical shell t is at least 0.0646 mm. It can be seen from this that if the metal material and the maximum operating temperature have been determined, then p and σ y are all constants, then the thickness t of the metal spherical shell is linearly proportional to the outer radius R of the spherical shell.

[0046] Please continue to refer to Figures 1 to 3 The present invention also provides a method for preparing an artificial aggregate, the method comprising the following steps:

[0047] Step S1, preparing a porous structure: using natural clay, industrial solid waste, and engineering waste as basic raw materials, and adding 1% to 10% by weight of powdered B4C or Gd2O3, adding water and a foaming agent to mix, and making particles, the specific mass ratio is as follows:

[0048]

[0049] The firing temperature is controlled at 1300°C for 3 hours; the particles are expanded by a foaming agent, and the internal moisture is released under the firing environment of 1300°C to obtain porous ceramsite. Finally, the obtained ceramsite is sieved and classified according to its size, cylinder pressure strength, and porosity to obtain a porous structure;

[0050] Step S2, soaking the porous structure: soaking the ceramsite prepared in step S1 in a water-based liquid. The open pores are the main channels for the ceramsite to absorb water. The liquid can enter the open pores through the action of surface tension and transfer inside the ceramsite through the connectivity of the pores. When the ceramsite absorbs the liquid to saturation, the volume of the water-based liquid can reach more than 25% of the total volume of the ceramsite.

[0051] Step S3, freezing the porous structure: grouping the ceramsite soaked in step S2 according to their sizes, and placing the grouped ceramsite into a freezer to freeze the outer layer liquid and lock the inner liquid;

[0052] Step S4, wrapping with metal shell: placing the ceramsite frozen in step S3 in a high temperature resistant scooping net, immersing it in the molten metal, and then scooping it out after the surface is wrapped with a layer of metal shell to obtain liquid-coated particles;

[0053] Step S5, completing post-processing: post-processing the liquid-coated particles obtained in step S4, i.e., cutting and separating the adhered artificial aggregates, reducing the defects of the metal shell by tempering, performing heating test and pressure resistance test on the obtained ceramsite, screening and obtaining qualified products, thereby obtaining artificial aggregates.

[0054] In this embodiment, more preferably, step S3 includes:

[0055] The size groups are separated according to the radius difference of 0.5 mm; and the average radius R corresponding to each group is determined in advance through experiments. 平均 , which satisfies the freezing time T required for the outer layer of liquid to freeze but the inner liquid to not freeze 冷冻 (R 平均 ) to prevent all liquid from freezing and cracking and destroying the porous structure; the unified freezing time of this group is taken as T 冷冻 (R 平均 ).

[0056] In this embodiment, more preferably, step S4 includes:

[0057] According to the different size groups, the average radius R of each group is determined in advance through experiments. 平均 The minimum soaking time T of ceramsite 浸泡 (R 平均 ), ensuring that its surface is covered with a metal shell with a thickness of t; the unified immersion time of this group is taken as T 浸泡 (R平均 ).

[0058] Specifically, three types of concrete test blocks were prepared for testing, namely artificial aggregate concrete (prepared by the aforementioned method, with the volume of natural water inside the aggregate reaching about 28%), ordinary concrete and serpentine concrete. The corresponding mix ratios are shown in the following table. The particle sizes of artificial coarse aggregate, ordinary crushed stone and serpentine are continuously graded from 5 to 10 mm, the fineness modulus of artificial fine aggregate, river sand and serpentine sand are all controlled at about 2.3, PO 52.5 silicate cement is selected, and the solid content of the water reducer is 28%.

[0059]

[0060] The concrete was formed into cylindrical test blocks with a diameter of 6 cm and a height of 4 cm, and the test was carried out after 28 days of standard curing. The three types of concrete were irradiated with neutrons of about 0.01eV, 1eV and 100eV energy through an electron accelerator, and the neutron shielding ability was judged by recording the flux after the neutrons penetrated the concrete. Each energy was irradiated for about 5 hours, and the neutron emission flux of the electron accelerator was about 100000n.

[0061] The neutron flux data after penetrating concrete is shown in the following table:

[0062] 0.01eV 1eV 100eV Artificial Aggregate Concrete 9253 13856 16966 Ordinary concrete 23698 35065 39745 Serpentine concrete 13959 22129 25678

[0063] It can be seen from the table that the neutron shielding ability of artificial aggregate concrete is better than that of ordinary concrete and serpentine concrete at three energies of 0.01eV, 1eV, and 100eV. The neutron shielding rate of artificial aggregate concrete can be increased by about 25% and 10% respectively compared with ordinary concrete and serpentine concrete.

[0064] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. The above embodiments only express several embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An artificial aggregate, characterized in that: include: A metal shell, wherein the metal shell is a sealed structure and is used to accommodate the porous structure; A porous structure, wherein the porous structure is formed into a prescribed shape by mixing ceramsite raw materials with 1% to 10% by weight of powdered B4C or Gd2O3, wherein the weight of B4C accounts for 20% to 80% of the total weight of the powder, and the particle size of the powder is 10 microns, and the formed body is dried and then fired; as well as The water-based liquid is natural water, tap water or boric acid solution contained in the pores of the porous structure.

2. The artificial aggregate according to claim 1, characterized in that: The porosity of the porous structure is greater than 30%, and the cylinder pressure strength is greater than 10 MPa.

3. The artificial aggregate according to claim 1, characterized in that: The ceramsite is at least one selected from aluminum oxide particles, silicon oxide particles, silicon carbide particles and silicon nitride particles.

4. The artificial aggregate according to claim 1, characterized in that: The metal shell is a metal spherical shell or other hollow special-shaped closed structure, and the metal is made of stainless steel.

5. The artificial aggregate according to claim 4, characterized in that: The outer radius of the metal spherical shell is R, and the thickness is t, wherein the value range of R is 1.5 mm to 20 mm. Where, α is the safety factor, which ranges from 1.5 to 2.0; p = 1.55 MPa is the critical boiling pressure of water at 200 °C; σ y =360MPa is the yield stress of the metal material.

6. The method for preparing artificial aggregate according to claim 5, characterized in that: The steps include: Step S1: using natural clay, industrial solid waste, and engineering waste as basic raw materials, and adding 1% to 10% by weight of powdered B4C or Gd2O3, wherein the weight of B4C accounts for 20% to 80% of the total weight of the powder, adding water and a foaming agent to mix and make particles, the specific mass ratio is as follows: The firing temperature was controlled at 1300°C for 3 h; The particles are expanded by a foaming agent, and the internal water is released under a firing environment of 1300°C to obtain porous ceramsite. Finally, the obtained ceramsite is screened and classified according to its size, cylinder pressure strength, and porosity. Step S2: soaking the ceramsite prepared in step S1 in a water-based liquid. The open pores are the main channels for the ceramsite to absorb water. The liquid can enter the open pores through the action of surface tension and transfer inside the ceramsite through the connectivity of the pores until the ceramsite absorbs the liquid to saturation and the volume of the water-based liquid reaches more than 25% of the total volume of the ceramsite. Step S3: grouping the ceramsite soaked in step S2 according to their sizes, and placing the grouped ceramsite into a freezer to freeze the outer layer of liquid and lock the inner liquid; Step S4: placing the ceramsite frozen in step S3 in a high temperature resistant scooping net, immersing it in the molten metal, and scooping it out after the surface is covered with a layer of metal shell to obtain liquid-coated particles; Step S5: post-processing the liquid-coated particles obtained in step S4, cutting and separating the adhered artificial aggregates, reducing the defects of the metal shell by tempering, performing heating tests and pressure tests on the obtained ceramsite, screening and obtaining qualified products, and obtaining artificial aggregates.

7. The preparation method according to claim 6, characterized in that: The step S3 comprises: The size groups are separated according to the radius difference of 0.5 mm; and the average radius R corresponding to each group is determined in advance through experiments. 平均 , which satisfies the freezing time T required for the outer layer of liquid to freeze but the inner liquid to not freeze 冷冻 (R 平均 ) to prevent all liquid from freezing and cracking and destroying the porous structure; the unified freezing time of this group is taken as T 冷冻 (R 平均 ).

8. The preparation method according to claim 6, characterized in that: The step S4 comprises: According to the different size groups, the average radius R of each group is determined in advance through experiments. 平均 The minimum soaking time T of ceramsite 浸泡 (R 平均 ), ensuring that its surface is covered with a metal shell with a thickness of t; The unified soaking time of this group is taken as T 浸泡 (R 平均 ).

Citation Information

Patent Citations

  • Cement-based neutron shielding material and preparation method thereof

    CN110415851A

  • Neutron radiation prevention boron carbide concrete and preparation method thereof

    CN114031353A

  • Preparation method of household garbage incineration bottom ash unfired porous artificial aggregate

    CN115466066A