Premixed concrete for building and preparation method thereof

By loading silicon and phosphorus elements and sulfide groups onto waste rubber tire particles, a synergistic flame retardant and antioxidant network is formed, which solves the problem of poor flame retardant and anti-aging properties of waste rubber tire concrete and achieves better overall performance.

CN118908643APending Publication Date: 2024-11-08NINGBO HANGZHOU BAY NEW AREA PUDONG CONCRETE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410810692.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When waste rubber tires are used as aggregate in concrete, the flame retardant and anti-aging properties of rubber concrete are significantly reduced.

Method used

Modified rubber particles loaded with silicon and phosphorus elements and sulfide groups are used. Through the synergistic effect of silicon and phosphorus elements, a silicon carbide protective layer is formed, which prevents heat and oxygen from entering during the combustion process. At the same time, the sulfide groups capture oxygen free radicals, stabilize the material structure, and delay the oxidation reaction.

Benefits of technology

It significantly improves the flame retardant and anti-aging properties of concrete, extending the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004906071940000071
    Figure BDA0004906071940000071
Patent Text Reader

Abstract

The invention relates to the technical field of cement-based building materials, in particular to premixed concrete for buildings and a preparation method of the premixed concrete. The invention discloses premixed concrete for buildings. The premixed concrete is prepared from the following raw materials in parts by weight: 200 to 300 parts of cement, 600 to 700 parts of machine-made sand, 50 to 60 parts of mineral powder, 40 to 60 parts of fly ash, 900 to 1100 parts of gravel, 120 to 150 parts of natural sand, 50 to 80 parts of modified rubber particles, 6 to 8 parts of water reducing agent and 150 to 170 parts of water, the modified rubber particles are waste rubber tire particles loaded with silicon and phosphorus elements and thioether groups. According to the premixed concrete for the building, the waste rubber tire particles serve as aggregate, waste rubber tires are effectively utilized, meanwhile, the problem of scarcity of building materials is solved to a certain degree, and meanwhile the defects that due to introduction of the rubber particles, the flame retardant property and the anti-aging property of the concrete are poor are effectively overcome through the modifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cement-based building materials, and more specifically, to a ready-mixed concrete for construction and a preparation method thereof. Background Art

[0002] In recent years, with the development of industrialization and urbanization, the global automobile industry has experienced rapid development. At the same time, the number of waste rubber tires has also increased. At present, waste rubber tires are usually disposed of by landfill or incineration, but the above methods will cause great waste of resources and environmental pollution.

[0003] In order to effectively improve the problem of difficult treatment of waste rubber tires, people thought of crushing waste rubber tires into particles and adding them to concrete as aggregates to make the concrete have better toughness and ductility. While effectively utilizing waste rubber tires, it also improves the problem of scarcity of building materials to a certain extent.

[0004] However, since rubber material is flammable and its anti-aging performance is relatively poorer than that of concrete itself, when waste rubber tire particles are added to concrete as aggregate, the flame retardant and anti-aging properties of the prepared rubber concrete will be significantly reduced. Summary of the invention

[0005] In order to improve the defects of rubber concrete, such as poor flame retardancy and anti-aging performance, the present application provides a ready-mixed concrete for construction and a preparation method thereof.

[0006] In a first aspect, the present application provides a ready-mixed concrete for construction, which adopts the following technical solution:

[0007] A ready-mixed concrete for construction comprises the following raw materials in parts by weight: 200-300 parts of cement, 600-700 parts of machine-made sand, 50-60 parts of mineral powder, 40-60 parts of fly ash, 900-1100 parts of crushed stone, 120-150 parts of natural sand, 50-80 parts of modified rubber particles, 6-8 parts of water reducing agent and 150-170 parts of water; the modified rubber particles are waste rubber tire particles loaded with silicon phosphorus elements and sulfide groups.

[0008] Silicon and phosphorus elements have a synergistic flame retardant effect. The mechanism is that silicon can play a flame retardant role by hindering heat conduction and mass transfer during the combustion process, thereby forming a silicon carbide protective layer to slow down the combustion rate, while phosphorus can play a flame retardant role by promoting the formation of a carbonized layer and improving the carbon soot structure, increasing the carbonization degree of the soot and preventing the entry of oxygen and heat.

[0009] When silicon and phosphorus are used together, silicon can promote the decomposition and activation of phosphorus, thereby improving the effect of phosphorus in the combustion process. At the same time, phosphorus can also improve the reactivity and effect of silicon, thus forming a synergistic flame retardant effect.

[0010] The thioether group has a certain antioxidant effect. The mechanism may be that the disulfide in the thioether group can capture and stabilize oxygen free radicals, that is, atoms or molecules with unpaired electrons in oxygen molecules, thereby reducing the concentration of free radicals, reducing the reaction between oxygen free radicals and material molecules, preventing free radicals from chain reactions in the system, delaying the progress of oxidation reactions, and reducing oxides to stable products, thereby extending the service life of the material and obtaining excellent anti-aging properties.

[0011] In summary, when waste rubber tire particles are loaded with silicon-phosphorus elements and sulfide groups, ready-mixed concrete will effectively compensate for the deterioration of flame retardancy and anti-aging properties caused by the introduction of waste rubber tires, thereby effectively improving the comprehensive performance of ready-mixed concrete.

[0012] Preferably, the modified rubber particles are composed of the following raw materials in parts by mass: 30-50 parts of waste rubber tire particles and 10-14 parts of a modifier, wherein the modifier includes a silane coupling agent, a flame retardant - trishydroxymethylphosphine oxide and a thioether-based antioxidant; the silane coupling agent is one of dichlorodimethylsilane, 3-chloropropyltriethoxysilane and vinyltriethoxysilane.

[0013] Preferably, the silane coupling agent is 3-chloropropyltriethoxysilane, and the 3-chloropropyltriethoxysilane is used in combination with the flame retardant-trihydroxymethylphosphine oxide, and the molar ratio of 3-chloropropyltriethoxysilane to the flame retardant-trihydroxymethylphosphine oxide is (1-3):1.

[0014] Preferably, the preparation method of the modifier is as follows: under nitrogen protection, trimethylolphosphine oxide is mixed with diethylene glycol dimethyl ether as a solvent, a hydrogen chloride absorption device and a drying tube are installed at the same time, 3-chloropropyltriethoxysilane is slowly added dropwise at a temperature of 20°C, the temperature is raised to 70-80°C within 1-2h after the addition is completed, the temperature is kept for 7-9h, and then the temperature is raised to 120-140°C, the reaction is performed for 5-7h, 0.5-0.7g of an acid binding agent is added, the pH value is adjusted to 5-6, the mixture is stirred sufficiently, and then filtered and distilled to obtain a solvent and a low-boiling-point substance, two volumes of deionized water and a 5wt% sodium carbonate solution are added, the pH value is adjusted to 7, the mixture is layered after stirring, the lower layer of liquid is taken out for drying and mixed with a thioether-based antioxidant to obtain a modifier.

[0015] When 3-chloropropyltriethoxysilane is selected as the coupling agent, and the molar ratio of 3-chloropropyltriethoxysilane to the flame retardant-trihydroxymethylphosphorus oxide is 2:1, the two hydroxyl groups on the trihydroxymethylphosphorus oxide can undergo a substitution reaction with 3-chloropropyltriethoxysilane and precipitate hydrogen chloride, thereby connecting 3-chloropropyltriethoxysilane to the main chain of trihydroxymethylphosphorus oxide. 3-chloropropyltriethoxysilane, as a coupling agent, links the waste rubber tire particles and the cement matrix, thereby forming a multi-party series network structure system, effectively reducing the possibility of deviation of the flame retardant-trihydroxymethylphosphorus oxide, and indirectly improving the flame retardant properties of ready-mixed concrete.

[0016] In addition, although both dichlorodimethylsilane and 3-chloropropyltriethoxysilane can react with trihydroxymethylphosphine oxide, the flame retardant effect obtained by dichlorodimethylsilane is relatively poor. The reason may be that the modifier prepared by using 3-chloropropyltriethoxysilane has a higher proportion of silicon element per unit mass. When the addition amount of dichlorodimethylsilane is too high, the hydroxyl groups on trihydroxymethylphosphine oxide will be completely replaced, thereby affecting the subsequent preparation of the modifier.

[0017] Preferably, the thioether-based antioxidant is one of di-n-octyl disulfide, bis(2-hydroxyethyl) disulfide and dicyclohexyl disulfide.

[0018] Preferably, the modifier also includes toluene-3,5-diisocyanate, the thioether-based antioxidant is bis(2-hydroxyethyl)disulfide, and the molar ratio of the 3-chloropropyltriethoxysilane, the flame retardant-trihydroxymethylphosphine oxide, toluene-3,5-diisocyanate and bis(2-hydroxyethyl)disulfide is (1-3):1:1:1.

[0019] Preferably, the preparation method of the modifier comprises the following steps:

[0020] S1. Under nitrogen protection, trimethylolphosphine oxide and solvent diethylene glycol dimethyl ether are mixed, and a hydrogen chloride absorption device and a drying tube are installed at the same time. 3-chloropropyltriethoxysilane is slowly added dropwise at a temperature of 20°C. After the addition is completed, the temperature is raised to 70-80°C within 1-2 hours, and the temperature is kept for 7-9 hours, and then the temperature is raised to 120-140°C, and the reaction is performed for 5-7 hours. 0.5-0.7g of an acid binding agent is added, and the pH value is adjusted to 5-6. After sufficient stirring, the mixture is filtered and distilled to obtain a solvent and a low-boiling-point substance, and two volumes of deionized water and a 5wt% sodium carbonate solution are added, and the pH value is adjusted to 7. After stirring, the mixture is separated into layers, and the lower layer of liquid is taken out for drying to obtain a flame retardant precursor.

[0021] S2. Mix the flame retardant precursor, bis(2-hydroxyethyl) disulfide, toluene-3,5-diisocyanate and N,N-dimethylformamide, then stir and mix at a temperature of 60-80° C., add dibutyltin dilaurate while stirring, and react for 6-10 hours to obtain a modifier.

[0022] When bis(2-hydroxyethyl) disulfide is selected as the thioether-based antioxidant and toluene-3,5-diisocyanate is added at the same time, the two isocyanate groups on toluene-3,5-diisocyanate can react and connect with the active hydroxyl groups on the flame retardant precursor and one hydroxyl group in bis(2-hydroxyethyl) disulfide, respectively, so that the flame retardant, antioxidant and coupling agent form a coupling network, effectively reduce the possibility of the antioxidant shifting, and further improve the anti-aging performance of ready-mixed concrete.

[0023] Preferably, the preparation method of the modified rubber particles is: mixing waste rubber tire particles with a modifier, and drying after the modifier is evenly attached to the waste rubber tire particles to obtain the modified rubber particles.

[0024] In a second aspect, the present application provides a method for preparing ready-mixed concrete for construction, which adopts the following technical solution:

[0025] A method for preparing ready-mixed concrete for construction comprises the following steps:

[0026] Step 1: Mix cement, fly ash, machine-made sand, crushed stone and natural sand to obtain a dry mixture;

[0027] Step 2: Add water, mineral powder, modified rubber particles and water reducing agent to the dry mixture, and then mix and stir at a temperature of 25-35° C. for 8-12 minutes to obtain ready-mixed concrete for construction.

[0028] In summary, this application has the following beneficial effects:

[0029] 1. Silicon and phosphorus have a synergistic flame retardant effect. The mechanism is that silicon can play a flame retardant role by hindering heat conduction and mass transfer in the combustion process, thereby forming a silicon carbide protective layer to slow down the combustion rate, while phosphorus can play a flame retardant role by promoting the formation of a carbonized layer and improving the structure of carbon smoke, increasing the carbonization degree of carbon smoke and preventing the entry of oxygen and heat; when silicon and phosphorus are used in combination, silicon can promote the decomposition and activation of phosphorus and improve the effect of phosphorus in the combustion process. At the same time, phosphorus can also improve the reactivity and effect of silicon, thus forming a synergistic flame retardant effect.

[0030] 2. The thioether group has a certain antioxidant effect. The mechanism may be that the disulfide in the thioether group can capture and stabilize oxygen free radicals, that is, atoms or molecules with unpaired electrons in oxygen molecules, thereby reducing the concentration of free radicals, reducing the reaction between oxygen free radicals and material molecules, preventing free radicals from chain reactions in the system, delaying the oxidation reaction, and reducing the oxides into stable products, thereby extending the service life of the material and obtaining excellent anti-aging properties.

[0031] 3. When bis(2-hydroxyethyl) disulfide is selected as the thioether-based antioxidant and toluene-3,5-diisocyanate is added at the same time, the two isocyanate groups on toluene-3,5-diisocyanate can react and connect with the active hydroxyl groups on the flame retardant precursor and one hydroxyl group in bis(2-hydroxyethyl) disulfide, respectively, so as to form a coupling network among the flame retardant, antioxidant and coupling agent, effectively reduce the possibility of the antioxidant shifting, and further improve the anti-aging performance of ready-mixed concrete. DETAILED DESCRIPTION

[0032] The present application is further described in detail below in conjunction with Examples 1-10 and Comparative Examples 1-2.

[0033] raw material

[0034] Cement P-O42.5; coarse sand in machine-made sand zone I; mineral powder S95; fly ash grade II; crushed stone 5-25mm; medium sand in natural sand zone II; water reducer polycarboxylic acid high-efficiency water reducer MT-3610; dichlorodimethylsilane CAS: 75-78-5; 3-chloropropyltriethoxysilane CAS: 5089-70-3; vinyltriethoxysilane CAS: 78-08-0; trihydroxymethylphosphine oxide CAS: 1067-12-5; acid binding agent-triethylamine CAS: 1 21-44-8; dioctyl disulfide CAS: 2690-08-6; bis(2-hydroxyethyl) disulfide CAS: 1892-29-1; dicyclohexyl disulfide CAS: 2550-40-5; toluene-3,5-diisocyanate CAS: 26471-62-5; N,N-dimethylformamide CAS: 68-12-2; dibutyltin dilaurate CAS: 77-58-7; diethylene glycol dimethyl ether CAS: 111-96-6.

[0035] Example

[0036] Example 1

[0037] A ready-mixed concrete for construction includes the following raw materials: 254kg of cement, 649kg of machine-made sand, 57kg of mineral powder, 50kg of fly ash, 1009kg of crushed stone, 137kg of natural sand, 65kg of modified rubber particles, 7kg of water reducing agent and 160kg of water, wherein the modified rubber particles are waste rubber tire particles loaded with silicon-phosphorus elements and sulfide groups.

[0038] The preparation method of ready-mixed concrete for construction comprises the following steps:

[0039] Step 1: Mix cement, fly ash, machine-made sand, crushed stone and natural sand to obtain a dry mixture;

[0040] Step 2: Add water, mineral powder, modified rubber particles and water reducing agent to the dry mixture, and then mix and stir at a temperature of 30° C. for 10 minutes to obtain ready-mixed concrete for construction.

[0041] The modified rubber particles include the following raw materials: 40 kg of waste rubber tire particles and 12 kg of modifier. It should be noted that the above addition amount represents the addition ratio;

[0042] The modifier includes a silane coupling agent, a flame retardant-trimethylolphosphine oxide and a thioether type anti-aging agent, and the molar ratio of the silane coupling agent, the flame retardant-trimethylolphosphine oxide and the thioether type anti-aging agent is 2:1:1; the silane coupling agent is 3-chloropropyltriethoxysilane, and the thioether type anti-aging agent is di-n-octyl disulfide;

[0043] The preparation method of the modifier is:

[0044] Under nitrogen protection, the flame retardant trihydroxymethylphosphine oxide is mixed with twice the volume of solvent diethylene glycol dimethyl ether, and a hydrogen chloride absorption device and a drying tube are installed at the same time. The silane coupling agent is slowly added at a temperature of 20°C. After the addition is completed, the temperature is raised to 75°C within 1.5 hours, kept warm for 8 hours, and then raised to 130°C, reacted for 6 hours, 0.6g of acid binding agent is added, the pH value is adjusted to between 5 and 6, and after sufficient stirring, the solvent and low boiling point products are obtained by suction filtration and distillation, and twice the volume of deionized water and 5wt% sodium carbonate solution are added, the pH value is adjusted to 7, and layers are separated after stirring. The lower layer of liquid is taken out for drying and mixed with a thioether-based antioxidant to obtain a modifier.

[0045] The preparation method of the modified rubber particles is as follows: waste rubber tire particles are mixed with a modifier, and after the modifier is uniformly attached to the waste rubber tire particles, the modified rubber particles are dried to obtain the modified rubber particles.

[0046] Example 2-3

[0047] The difference from Example 1 is that the addition amount of each component of the ready-mixed concrete for construction is different, as shown in Table 1.

[0048] Table 1 Addition amount of each component of ready-mixed concrete for construction in Examples 1-3 / kg

[0049]

[0050] Example 4

[0051] The difference from Example 1 is that dichlorodimethylsilane is used as the silane coupling agent.

[0052] Example 5

[0053] The difference from Example 1 is that the silane coupling agent is vinyltriethoxysilane.

[0054] Example 6

[0055] The difference from Example 1 is that the molar ratio of 3-chloropropyltriethoxysilane, the flame retardant trishydroxymethylphosphine oxide and the thioether type antioxidant is 1:1:1.

[0056] Example 7

[0057] The difference from Example 1 is that the molar ratio of 3-chloropropyltriethoxysilane, flame retardant trishydroxymethylphosphine oxide and thioether type antioxidant is 3:1:1.

[0058] Example 8

[0059] The difference from Example 1 is that toluene-3,5-diisocyanate is also added to the modifier, and the molar ratio of 3-chloropropyltriethoxysilane, flame retardant-trishydroxymethylphosphine oxide, toluene-3,5-diisocyanate and di-n-octyl disulfide is 2:1:1:1;

[0060] The preparation method of the modifier comprises the following steps:

[0061] S1. Under nitrogen protection, trimethylolphosphine oxide was mixed with twice the volume of diethylene glycol dimethyl ether, and a hydrogen chloride absorption device and a drying tube were installed. 3-chloropropyltriethoxysilane was slowly added dropwise at a temperature of 20°C. After the addition was completed, the temperature was raised to 75°C within 1.5 hours, and the temperature was kept for 8 hours, and then the temperature was raised to 130°C, and the reaction was performed for 5-7 hours. 0.6 g of an acid binding agent was added, and the pH value was adjusted to between 5 and 6. After sufficient stirring, the mixture was filtered and distilled to obtain a solvent and a low-boiling-point substance. Two volumes of deionized water and a 5wt% sodium carbonate solution were added, and the pH value was adjusted to 7. After stirring, the mixture was separated into layers, and the lower layer of liquid was taken out for drying to obtain a flame retardant precursor.

[0062] S2. Mix the flame retardant precursor, di-n-octyl disulfide, toluene-3,5-diisocyanate and N,N-dimethylformamide, then stir and mix at 70° C., add 2 wt % dibutyltin dilaurate while stirring, and react for 8 hours to obtain a modifier.

[0063] Example 9

[0064] The difference from Example 8 is that the sulfide-based antioxidant is bis(2-hydroxyethyl) disulfide.

[0065] Example 10

[0066] The difference from Example 8 is that dicyclohexyl disulfide is used as the sulfide-type antioxidant.

[0067] Comparative Example

[0068] Comparative Example 1

[0069] The difference from Example 1 is that the modified rubber particles are replaced by the same amount of waste rubber particles.

[0070] Comparative Example 2

[0071] The difference from Example 1 is that no thioether type antioxidant is added to the modifier.

[0072] Performance testing

[0073] Detection Methods

[0074] 1. Flame retardant performance test

[0075] Ten samples were taken out from Examples 1-7 and Comparative Example 1 and cured. After curing, they were placed in a natural environment for 90 days. Then, the fire resistance of the samples was tested according to TEK7-1C 2009 "Fire resistance of concrete block components" and the average value was taken. The test results are shown in Table 2.

[0076] Table 2 Fire resistance limit of Examples 1-7 and Comparative Example 1

[0077] Fire resistance Fire resistance Example 1 4 hours 12 minutes Example 5 3 hours 41 minutes Example 2 4 hours 10 minutes Example 6 4 hours 04 minutes Example 3 4 hours 02 minutes Example 7 3 hours 57 minutes Example 4 3 hours 50 minutes Comparative Example 1 3 hours 05 minutes

[0078] 2. Anti-aging performance test

[0079] Six samples were taken from Example 1, Examples 8-10 and Comparative Example 2 respectively and cured. After curing, they were placed in a natural environment for 90 days. Then, three of the samples were tested for compressive properties according to GB / T 50081-2002 "Compressive Test Method for Concrete and Its Products", and the original compressive strength was obtained and the average value was taken.

[0080] The other three samples were then placed in an aerobic environment at 400°C for 24 hours, and the compressive properties of the samples after thermal oxidation treatment were tested to obtain the compressive strength after oxygen treatment and take the average value, and finally calculate the aging percentage; aging percentage = (original compressive strength-compressive strength after oxygen treatment) / original compressive strength × 100%.

[0081] The test data are shown in Table 3.

[0082] Table 3 Anti-aging performance of Example 1, Examples 8-10 and Comparative Example 1

[0083] Aging percentage Aging percentage Example 1 10.1% Example 10 8.8% Example 8 9.4% Comparative Example 2 28.9% Example 9 4.3%

[0084] Referring to Examples 1-3 and Comparative Example 1 and in combination with Table 2, it can be seen that the fire resistance limits of Examples 1-3 are significantly improved compared with Comparative Example 1, which shows that the use of the modifier can enable the concrete to still have excellent flame retardant properties after adding waste rubber tire particles.

[0085] The reason is that the modifier contains silane coupling agent and flame retardant - trihydroxymethyl phosphorus oxide. The silicon and phosphorus elements have a synergistic flame retardant effect. The mechanism is that the silicon element can play a flame retardant role by hindering heat conduction and mass transfer during the combustion process, thereby forming a layer of silicon carbide protective layer to slow down the combustion rate, while the phosphorus element can play a flame retardant role by promoting the formation of a carbonized layer and improving the carbon soot structure, increasing the carbonization degree of the carbon soot and preventing the entry of oxygen and heat.

[0086] When silicon and phosphorus are used together, silicon can promote the decomposition and activation of phosphorus, thereby improving the effect of phosphorus in the combustion process. At the same time, phosphorus can also improve the reactivity and effect of silicon, thus forming a synergistic flame retardant effect.

[0087] Compared with Example 1, the fire resistance limits of Examples 2-3 are relatively low, which indicates that when the components of the ready-mixed concrete for construction are added in the amounts of Example 1, the prepared ready-mixed concrete for construction will have relatively better flame retardant properties.

[0088] With reference to Example 1 and Examples 4-5 and in combination with Table 2, it can be seen that, relative to Example 1, the fire resistance limit of Example 4 is significantly reduced, while the fire resistance limit of Example 5 is further reduced. This shows that among 3-chloropropyltriethoxysilane, dichlorodimethylsilane and vinyltriethoxysilane, when 3-chloropropyltriethoxysilane is selected as the silane coupling agent, the prepared ready-mixed concrete for construction will have the relatively best flame retardant properties, followed by dichlorodimethylsilane, and vinyltriethoxysilane.

[0089] The reason is that when dichlorodimethylsilane or 3-chloropropyltriethoxysilane is used as the coupling agent, the chloride ions on the dichlorodimethylsilane or 3-chloropropyltriethoxysilane can undergo substitution reaction with the two hydroxyl groups on trimethylolphosphine oxide and precipitate hydrogen chloride, thereby connecting the dichlorodimethylsilane or 3-chloropropyltriethoxysilane to the main chain of trimethylolphosphine oxide, and the dichlorodimethylsilane or 3-chloropropyltriethoxysilane as a coupling agent links the waste rubber tire particles and the cement matrix, thereby forming a multi-party series network structure system, effectively reducing the possibility of deviation of the flame retardant-trimethylolphosphine oxide, and indirectly improving the flame retardant properties of ready-mixed concrete.

[0090] Among them, although both dichlorodimethylsilane and 3-chloropropyltriethoxysilane can react with trihydroxymethylphosphine oxide, the flame retardant effect obtained by dichlorodimethylsilane is relatively poor. The reason may be that, per unit mass, the modifier prepared by using 3-chloropropyltriethoxysilane has a higher proportion of silicon element, and when the addition amount of dichlorodimethylsilane is too high, the hydroxyl groups on trihydroxymethylphosphine oxide will be completely replaced, thereby affecting the subsequent preparation of the modifier.

[0091] With reference to Example 1 and Examples 6-7 and in combination with Table 2, it can be seen that the fire resistance limits of Examples 6-7 are slightly reduced relative to Example 1, which indicates that when the molar ratio of 3-chloropropyltriethoxysilane, flame retardant-trihydroxymethylphosphine oxide and thioether-type antioxidant is adopted in Example 1, the prepared ready-mixed concrete for construction will have better flame retardant properties.

[0092] Referring to Example 1 and Comparative Example 2 and in combination with Table 3, it can be seen that the aging percentage of Example 1 is significantly reduced compared with Comparative Example 2, which shows that the addition of thioether-type antioxidant can still have excellent anti-aging performance after waste rubber tire particles are added to ready-mixed concrete for construction.

[0093] The reason is that the sulfide group has a certain antioxidant effect. The mechanism may be that the disulfide in the sulfide group can capture and stabilize oxygen free radicals, that is, atoms or molecules with unpaired electrons in oxygen molecules, thereby reducing the concentration of free radicals, reducing the reaction of oxygen free radicals with material molecules, preventing free radicals from chain reactions in the system, delaying the progress of oxidation reactions, and reducing oxides into stable products, thereby extending the service life of the material and obtaining excellent anti-aging properties.

[0094] Referring to Examples 8-10 and in combination with Table 3, it can be seen that, relative to Example 9, the aging percentages of Examples 8 and 10 are significantly improved, which indicates that, under the premise of using toluene-3,5-diisocyanate, when bis(2-hydroxyethyl)disulfide is selected among di-n-octyl disulfide, bis(2-hydroxyethyl)disulfide and dicyclohexyl disulfide, the prepared ready-mixed concrete for construction will have better anti-aging performance.

[0095] The reason is that when bis(2-hydroxyethyl) disulfide is selected as the sulfide-based antioxidant and toluene-3,5-diisocyanate is added at the same time, the two isocyanate groups on toluene-3,5-diisocyanate can react and connect with the active hydroxyl groups on the flame retardant precursor and one hydroxyl group in bis(2-hydroxyethyl) disulfide respectively, prompting the flame retardant, antioxidant and coupling agent to form a coupling network, effectively reducing the possibility of the antioxidant shifting, and further improving the anti-aging performance of ready-mixed concrete.

[0096] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A ready-mixed concrete for construction, characterized in that: The invention comprises the following raw materials in parts by weight: 200-300 parts of cement, 600-700 parts of machine-made sand, 50-60 parts of mineral powder, 40-60 parts of fly ash, 900-1100 parts of crushed stone, 120-150 parts of natural sand, 50-80 parts of modified rubber particles, 6-8 parts of water reducing agent and 150-170 parts of water; the modified rubber particles are waste rubber tire particles loaded with silicon phosphorus elements and sulfide groups.

2. The ready-mixed concrete for construction according to claim 1, characterized in that: The modified rubber particles are composed of the following raw materials in parts by mass: 30-50 parts of waste rubber tire particles and 10-14 parts of a modifier, wherein the modifier includes a silane coupling agent, a flame retardant-trihydroxymethylphosphine oxide and a thioether-based anti-aging agent; the silane coupling agent is one of dichlorodimethylsilane, 3-chloropropyltriethoxysilane and vinyltriethoxysilane.

3. The ready-mixed concrete for construction according to claim 2, characterized in that: The silane coupling agent is 3-chloropropyltriethoxysilane, which is used in combination with the flame retardant trihydroxymethylphosphine oxide, and the molar ratio of 3-chloropropyltriethoxysilane to the flame retardant trihydroxymethylphosphine oxide is (1-3):

1.

4. The ready-mixed concrete for construction according to claim 3, characterized in that: The preparation method of the modifier comprises the following steps: under nitrogen protection, trimethylolphosphine oxide is mixed with diethylene glycol dimethyl ether as a solvent, a hydrogen chloride absorption device and a drying tube are installed at the same time, 3-chloropropyltriethoxysilane is slowly added dropwise at a temperature of 20°C, the temperature is raised to 70-80°C within 1-2 hours after the addition is completed, the temperature is kept for 7-9 hours, and then the temperature is raised to 120-140°C, the reaction is performed for 5-7 hours, 0.5-0.7g of an acid binding agent is added, the pH value is adjusted to 5-6, the mixture is stirred sufficiently, and then the mixture is filtered and distilled to obtain a solvent and a low-boiling-point substance, two volumes of deionized water and a 5wt% sodium carbonate solution are added, the pH value is adjusted to 7, the mixture is layered after stirring, the lower layer of liquid is taken out for drying and mixed with a thioether-based anti-aging agent to obtain the modifier.

5. The ready-mixed concrete for construction according to claim 3, characterized in that: The preparation method of the modifier is as follows: the thioether-based anti-aging agent is one of di-n-octyl disulfide, bis(2-hydroxyethyl) disulfide and dicyclohexyl disulfide.

6. The ready-mixed concrete for construction according to claim 5, characterized in that: The modifier also includes toluene-3,5-diisocyanate, the thioether-based antioxidant is bis(2-hydroxyethyl)disulfide, and the molar ratio of the 3-chloropropyltriethoxysilane, the flame retardant-trihydroxymethylphosphine oxide, toluene-3,5-diisocyanate and bis(2-hydroxyethyl)disulfide is (1-3):1:1:

1.

7. The ready-mixed concrete for construction according to claim 6, characterized in that: The preparation method of the modifier comprises the following steps: S1. Under nitrogen protection, trimethylolphosphine oxide and solvent diethylene glycol dimethyl ether are mixed, and a hydrogen chloride absorption device and a drying tube are installed at the same time. 3-chloropropyltriethoxysilane is slowly added dropwise at a temperature of 20°C. After the addition is completed, the temperature is raised to 70-80°C within 1-2 hours, and the temperature is kept for 7-9 hours, and then the temperature is raised to 120-140°C, and the reaction is performed for 5-7 hours. 0.5-0.7g of an acid binding agent is added, and the pH value is adjusted to 5-6. After sufficient stirring, the mixture is filtered and distilled to obtain a solvent and a low-boiling-point substance, and two volumes of deionized water and a 5wt% sodium carbonate solution are added, and the pH value is adjusted to 7. After stirring, the mixture is separated into layers, and the lower layer of liquid is taken out for drying to obtain a flame retardant precursor. S2. Mix the flame retardant precursor, bis(2-hydroxyethyl) disulfide, toluene-3,5-diisocyanate and N,N-dimethylformamide, then stir and mix at a temperature of 60-80° C., add dibutyltin dilaurate while stirring, and react for 6-10 hours to obtain a modifier.

8. The ready-mixed concrete for construction according to claim 1, characterized in that: The preparation method of the modified rubber particles comprises: mixing waste rubber tire particles with a modifier, and drying the waste rubber tire particles after the modifier is evenly attached to the waste rubber tire particles to obtain the modified rubber particles.

9. A method for preparing ready-mixed concrete for construction according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Mix cement, fly ash, machine-made sand, crushed stone and natural sand to obtain a dry mixture; Step 2: Add water, mineral powder, modified rubber particles and water reducing agent to the dry mixture, and then mix and stir at a temperature of 25-35° C. for 8-12 minutes to obtain ready-mixed concrete for construction.

Citation Information

Patent Citations

  • Phosphor-silicon-containing aggregated flame retardant and preparation method thereof

    CN107266685A

  • Impermeable concrete and preparation method thereof

    CN111704403A

  • High-temperature-resistant anticracking concrete and preparation method thereof

    CN111925160A

  • High-temperature-resistant flame-retardant explosion-proof high-strength concrete and preparation method thereof

    CN113121174A

  • Self-compacting concrete

    CN115650651A