High-performance concrete and preparation method thereof

A high-performance concrete preparation method using a specific ratio of cement, mineral admixtures, coarse aggregate, fine aggregate, and modified polypropylene fiber has solved the problem of insufficient durability of traditional concrete, achieving high tensile strength and crack resistance, and improving the durability and safety of engineering structures.

CN118908649APending Publication Date: 2024-11-08SHAANXI HENGSHENG GREEN CONSTRUCTION TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410957235.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional concrete is not durable enough in large-scale, complex projects with greater environmental adaptability. It has low tensile strength, poor resistance to deformation, and poor crack resistance, which affects the structural safety and service life.

Method used

High-performance concrete is prepared by mixing and curing cement, mineral admixtures, coarse aggregate, fine aggregate, modified polypropylene fiber, and polyethylene glycol-modified aliphatic epoxy resin in a specific ratio, thereby improving durability, tensile strength, and crack resistance.

Benefits of technology

The prepared high-performance concrete has good durability, high tensile strength, strong deformation resistance, and good crack resistance, which extends the service life of the structure and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949218230000041
    Figure BDA0004949218230000041
  • Figure BDA0004949218230000051
    Figure BDA0004949218230000051
  • Figure BDA0004949218230000061
    Figure BDA0004949218230000061
Patent Text Reader

Abstract

The invention relates to the technical field of concrete. The invention discloses high-performance concrete and a preparation method thereof. The concrete is prepared from the following raw materials: cement, a mineral admixture, coarse aggregate, fine aggregate, a polycarboxylic acid water reducing agent, modified polypropylene fiber, water and polyethylene glycol modified aliphatic epoxy resin. The preparation method comprises the following steps: mixing and stirring coarse aggregate, fine aggregate, mineral admixture and modified polypropylene fiber to prepare a premix; adding cement, a polycarboxylate superplasticizer, water and polyethylene glycol modified aliphatic epoxy resin into the premix, mixing and stirring to obtain a concrete mixture; and injecting the concrete mixture into a mold for molding, curing and demolding to obtain the high-performance concrete. The prepared high-performance concrete is good in durability, high in tensile strength, good in deformation resistance and good in crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of concrete technology, and in particular to a high performance concrete and a preparation method thereof. Background Art

[0002] With the rapid development of global infrastructure construction, concrete, as a basic building material, has received extensive attention. Ordinary concrete is a composite material composed of cementitious materials and aggregates. Generally, cement is used as the main cementitious material, sand and gravel are used as aggregates, and chemical admixtures and mineral admixtures are added when necessary. According to a certain ratio, the finished product is obtained through mixing, compacting, and curing and hardening. It is widely used in engineering fields such as bridge construction, house construction, and road construction.

[0003] Traditional concrete technology has undergone a long period of development and optimization, and it has performed stably in most conventional construction projects. However, as projects move towards larger, more complex and more environmentally adaptable directions, traditional concrete can no longer meet the requirements. The main problems include insufficient durability. If concrete is exposed to harsh environments for a long time, such as acid rain, salt spray, and freeze-thaw cycles, it is easy to cause corrosion and spalling of concrete, shortening its service life; low tensile strength, which limits the application of concrete in complex structures under stress; poor deformation resistance and crack resistance, which makes concrete prone to cracks when subjected to tension or temperature stress changes, affecting structural safety and durability. These performance defects not only increase maintenance costs, but may also pose a potential threat to public safety.

[0004] Therefore, there is an urgent need to develop a high-performance concrete with good durability, high tensile strength, good deformation resistance and good crack resistance. Summary of the invention

[0005] In order to solve at least one of the above technical problems, a high-performance concrete with good durability, high tensile strength, good deformation resistance and good crack resistance is developed. The present application provides a high-performance concrete and a preparation method thereof.

[0006] On the one hand, the present application provides a high-performance concrete, whose raw material composition includes, by weight: 400-500 parts of cement, 120-300 parts of mineral admixture, 900-1000 parts of coarse aggregate, 600-750 parts of fine aggregate, 5-10 parts of polycarboxylic acid water-reducing agent, 5-10 parts of modified polypropylene fiber, 120-150 parts of water, and 8-15 parts of polyethylene glycol-modified aliphatic epoxy resin.

[0007] By adopting the above technical solution, the present application adopts specific raw materials and proportions to produce high-performance concrete with good durability, high tensile strength, good deformation resistance and good crack resistance.

[0008] The application adds mineral admixtures, which can effectively reduce the hydration heat, improve the later strength of concrete, and enhance durability. The addition of modified polypropylene fiber can enhance the crack resistance and toughness of concrete, and has a significant effect on preventing early plastic shrinkage cracks and improving impact resistance. The addition of polyethylene glycol-modified aliphatic epoxy resin can increase the density of concrete, thereby improving the overall durability and mechanical properties.

[0009] Optionally, the raw material composition includes, by weight: 420-480 parts of cement, 160-260 parts of mineral admixture, 920-980 parts of coarse aggregate, 650-700 parts of fine aggregate, 7-8 parts of polycarboxylic acid water reducer, 7-8 parts of modified polypropylene fiber, 130-140 parts of water, and 10-13 parts of polyethylene glycol-modified aliphatic epoxy resin.

[0010] Optionally, the raw material composition includes, by weight: 450 parts of cement, 210 parts of mineral admixture, 950 parts of coarse aggregate, 680 parts of fine aggregate, 7.5 parts of polycarboxylic acid water-reducing agent, 7.5 parts of modified polypropylene fiber, 135 parts of water, and 11.5 parts of polyethylene glycol-modified aliphatic epoxy resin.

[0011] Optionally, the cement is P.O42.5 ordinary Portland cement.

[0012] Optionally, the mineral admixtures are fly ash and silica ash, and the weight ratio of the fly ash to the silica ash is 4 to 10:1.

[0013] By adopting the above technical solution, fly ash can significantly improve the working performance of concrete and reduce the hydration heat, while silica fume has extremely high volcanic ash activity and can significantly improve the later strength and durability of concrete. The two can be mixed in a certain proportion to achieve complementary performance and improve the durability, tensile strength, deformation resistance and crack resistance of concrete.

[0014] Optionally, the coarse aggregate is a secondary grade crushed stone of 5 to 10 mm and 16 to 25 mm, with a mixing ratio of 1:2 to 3.

[0015] By adopting the above technical solution, the grading of coarse aggregate can form a good particle grading distribution, ensure low aggregate void ratio in concrete, improve the density of concrete, improve the mechanical properties of concrete and reduce the tendency of cracking.

[0016] Optionally, the fine aggregate is river sand with a fineness modulus of 2.6 to 2.9.

[0017] By adopting the above technical solutions, fine aggregate can reduce the porosity inside concrete, improve the concrete's impermeability and freeze-thaw resistance, thereby enhancing the durability of concrete and extending the service life of the structure. Fine aggregate also helps control the concrete's autogenous shrinkage and shrinkage, reduce cracks caused by water evaporation and volume changes during cement hydration, and thus improve the concrete's resistance to deformation and cracking.

[0018] Optionally, the modified polypropylene fiber is prepared by: dispersing vinyl triethoxysilane in a solvent to obtain a vinyl triethoxysilane solution; immersing polypropylene fiber in the vinyl triethoxysilane solution for 30 to 60 minutes, and drying to obtain the modified polypropylene fiber.

[0019] By adopting the above technical solution, the modified polypropylene fiber can enhance the crack resistance and deformation resistance of concrete, improve durability, and extend the service life of the concrete structure.

[0020] Optionally, the vinyltriethoxysilane accounts for 0.5-2 wt % of the polypropylene fiber.

[0021] By adopting the above technical solution, the vinyl triethoxysilane of the present application can effectively cover the surface of the polypropylene fiber to form a dense silane protective film. Too low a concentration may result in an incomplete modified layer, affecting the bonding effect between the fiber and the concrete matrix; while too high a concentration may cause a waste of resources.

[0022] Optionally, the polyethylene glycol-modified aliphatic epoxy resin is prepared by polyethylene glycol and an aliphatic epoxy resin, and the weight ratio of the polyethylene glycol to the aliphatic epoxy resin is 1:3-5.

[0023] By adopting the above technical solution, the polyethylene glycol-modified aliphatic epoxy resin of the present application can improve the deformation resistance and crack resistance of concrete and improve durability.

[0024] Optionally, the molecular weight of the aliphatic epoxy resin is 600-1000, and the epoxy equivalent of the aliphatic epoxy resin is 150-200 g / Eq.

[0025] By adopting the above technical solution, the molecular weight and epoxy equivalent of the aliphatic epoxy resin of the present application can balance the processing performance and mechanical properties of the resin.

[0026] In a second aspect, the present application provides a method for preparing the above-mentioned high performance concrete, comprising the following steps: S1. Mixing and stirring the coarse aggregate, fine aggregate, mineral admixture and modified polypropylene fiber in the formula amount to prepare a premix; S2, adding cement, polycarboxylate water-reducing agent, water, polyethylene glycol-modified aliphatic epoxy resin to the premix, mixing and stirring to obtain a concrete mixture; S3, injecting the concrete mixture into a mold for molding, curing, and demoulding to obtain the high performance concrete.

[0027] By adopting the above technical solution, the preparation method adopted in this application has a simple process and is environmentally friendly and pollution-free during the preparation process. The gradual addition of raw materials in this application is conducive to regulating the performance of concrete, avoiding side reactions and adverse effects, and the high-performance concrete prepared has good durability, high tensile strength, good deformation resistance and good crack resistance.

[0028] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application adopts specific raw materials and proportions to produce high-performance concrete with good durability, high tensile strength, good deformation resistance and good crack resistance.

[0029] 2. The addition of modified polypropylene fiber in this application can enhance the crack resistance and toughness of concrete, and has a significant effect on preventing early plastic shrinkage cracks and improving impact resistance. The addition of polyethylene glycol-modified aliphatic epoxy resin can increase the density of concrete, thereby improving the overall durability and mechanical properties.

[0030] 3. The preparation method adopted in this application has a simple process and is environmentally friendly and pollution-free during the preparation process. The gradual addition of raw materials in this application is conducive to regulating the performance of concrete, avoiding side reactions and adverse effects, and the high-performance concrete prepared has good durability, high tensile strength, good deformation resistance and good crack resistance. DETAILED DESCRIPTION

[0031] The present application is further described in detail below in conjunction with embodiments.

[0032] The present application designs a high-performance concrete, whose raw material composition includes, by weight: 400-500 parts of cement, 120-300 parts of mineral admixture, 900-1000 parts of coarse aggregate, 600-750 parts of fine aggregate, 5-10 parts of polycarboxylic acid water-reducing agent, 5-10 parts of modified polypropylene fiber, 120-150 parts of water, and 8-15 parts of polyethylene glycol-modified aliphatic epoxy resin.

[0033] The high performance concrete of the present application is prepared by the following method, comprising the following steps: S1. Mixing and stirring the coarse aggregate, fine aggregate, mineral admixture and modified polypropylene fiber in the formula amount to prepare a premix; S2, adding cement, polycarboxylate water-reducing agent, water, polyethylene glycol-modified aliphatic epoxy resin to the premix, mixing and stirring to obtain a concrete mixture; S3, injecting the concrete mixture into a mold for molding, curing, and demoulding to obtain the high performance concrete.

[0034] The applicant has designed the technical solution of the present application in view of the problems of existing concrete such as insufficient durability, low tensile strength, poor deformation resistance and poor crack resistance.

[0035] The high performance concrete prepared in the present application has good durability, high tensile strength, good deformation resistance and good crack resistance. The preparation method adopted in the present application has a simple process and is environmentally friendly and pollution-free during the preparation process.

[0036] The raw materials used in this application are as follows: Fly ash: Wuhan Lianhekang Biotechnology Co., Ltd., product number: A01085.

[0037] Silica fume: Shandong Yonglida New Material Technology Co., Ltd., purity: 99%.

[0038] Vinyltriethoxysilane: CAS: 78-08-0.

[0039] Ethanol: CAS: 64-17-5.

[0040] Polypropylene fiber: Shandong Yonglida New Material Technology Co., Ltd., specification: 19mm.

[0041] Polyethylene glycol: CAS: 25322-68-3. Specific embodiments

[0042] Embodiments 1 to 5 The specific raw material weights of the high performance concrete prepared in Examples 1 to 5 are shown in Table 1.

[0043] Table 1 Among them, cement is P.O42.5 ordinary Portland cement; The mineral admixtures are fly ash and silica fume, and the weight ratio of fly ash to silica fume is 7:1; The coarse aggregate is 5-10mm and 16-25mm secondary grade crushed stone, with a mixing ratio of 1:2; the fine aggregate is river sand with a fineness modulus of 2.8; the polycarboxylate water reducer is Sika 540P (Sika, Switzerland); The preparation method of modified polypropylene fiber is as follows: dispersing vinyl triethoxysilane in a solvent to obtain a vinyl triethoxysilane solution; immersing polypropylene fiber in the vinyl triethoxysilane solution for 45 minutes, and drying to obtain modified polypropylene fiber; the vinyl triethoxysilane accounts for 1wt% of the polypropylene fiber.

[0044] The polyethylene glycol-modified aliphatic epoxy resin is prepared by polyethylene glycol and aliphatic epoxy resin, wherein the weight ratio of polyethylene glycol to aliphatic epoxy resin is 1:4; the molecular weight of the aliphatic epoxy resin is 800, and the epoxy equivalent is 170 g / Eq.

[0045] The method for preparing high performance concrete comprises the following steps: S1. Mix and stir the formulated amount of coarse aggregate, fine aggregate, mineral admixture, and modified polypropylene fiber to prepare a premix; S2, adding cement, polycarboxylate water-reducing agent, water, polyethylene glycol-modified aliphatic epoxy resin into the premix, mixing and stirring to obtain a concrete mixture; S3, injecting concrete mixture into the mold for shaping, curing, and demoulding to obtain high performance concrete.

[0046] Except for the weight of raw materials, the rest of Examples 2 to 5 are the same as Example 1.

[0047] Comparative Examples 1 to 4 Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that modified polypropylene fiber and polyethylene glycol-modified aliphatic epoxy resin are not added in Comparative Example 1.

[0048] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that no modified polypropylene fiber is added in Comparative Example 2.

[0049] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that the polyethylene glycol-modified aliphatic epoxy resin is not added in Comparative Example 3.

[0050] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that the preparation method of the high performance concrete of Comparative Example 4 is: S1, mixing and stirring all raw materials to obtain a concrete mixture; S2. Inject the concrete mixture into a mold for molding, curing, and demoulding to obtain high-performance concrete.

[0051] Experimental testing Test items and test methods Durability testing: According to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the carbonation depth of concrete is tested to assess its durability.

[0052] Tensile strength test: The splitting tensile strength of concrete is measured according to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".

[0053] Deformation resistance test: According to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the creep coefficient of concrete is tested to evaluate its deformation resistance.

[0054] Crack resistance test: Place a flat thin plate high performance concrete precast part with a size of 800mm×600mm×100mm in a 100℃ oven for 28 days and observe whether there are cracks.

[0055] The high performance concrete prepared in Examples 1 to 5 and Comparative Examples 1 to 4 was tested for durability, tensile strength, deformation resistance and crack resistance. The test results are shown in Table 2.

[0056] Table 2 From the test results in Table 2, it can be seen that the high performance concrete prepared in Examples 1 to 5 has good durability, high tensile strength, good deformation resistance and good crack resistance.

[0057] Comparative Example 1 did not add modified polypropylene fiber and polyethylene glycol-modified aliphatic epoxy resin, and Comparative Example 2 did not add modified polypropylene fiber; Comparative Example 3 did not add polyethylene glycol-modified aliphatic epoxy resin. The durability, tensile strength, deformation resistance and crack resistance of the high-performance concrete prepared in Comparative Examples 1 to 3 were significantly reduced.

[0058] The durability, tensile strength, deformation resistance and crack resistance of the high performance concrete prepared in Comparative Example 4 are all inferior to those in Example 3.

[0059] Embodiments 6 to 13 Example 6 The difference between Example 6 and Example 3 is that in Example 6, the weight ratio of fly ash to silica ash is 4:1.

[0060] Example 7 The difference between Example 7 and Example 3 is that in Example 7, the weight ratio of fly ash to silica fume is 10:1.

[0061] Example 8 The difference between Example 8 and Example 3 is that in Example 8, the coarse aggregate is 5-10 mm and 16-25 mm secondary graded crushed stone, and the mixing ratio is 1:2.5.

[0062] Example 9 The difference between Example 9 and Example 3 is that in Example 9, the coarse aggregate is 5-10 mm and 16-25 mm secondary graded crushed stone, and the mixing ratio is 1:3.

[0063] Example 10 The difference between Example 10 and Example 3 is that in the polyethylene glycol-modified aliphatic epoxy resin of Example 10, the weight ratio of polyethylene glycol to aliphatic epoxy resin is 1:3.

[0064] Embodiment 11 The difference between Example 11 and Example 3 is that in the polyethylene glycol-modified aliphatic epoxy resin of Example 11, the weight ratio of polyethylene glycol to aliphatic epoxy resin is 1:5.

[0065] Example 12 The difference between Example 12 and Example 3 is that in the polyethylene glycol-modified aliphatic epoxy resin of Example 12, the molecular weight of the aliphatic epoxy resin is 600, and the epoxy equivalent is 150 g / Eq.

[0066] Example 13 The difference between Example 13 and Example 3 is that in the polyethylene glycol-modified aliphatic epoxy resin of Example 13, the molecular weight of the aliphatic epoxy resin is 1000 and the epoxy equivalent is 200 g / Eq.

[0067] The high performance concrete prepared in Examples 6 to 13 was tested for durability, tensile strength, deformation resistance and crack resistance. The test results are shown in Table 3.

[0068] Table 3 From the test results in Table 3, it can be seen that the difference between Example 6 and Example 7 and Example 3 is that the weight ratio of fly ash to silica fume is different. Among them, the high-performance concrete prepared in Example 3 has the best durability, tensile strength and deformation resistance.

[0069] The difference between Example 8 and Example 9 and Example 3 is that the mixing ratio of the secondary crushed stone in the coarse aggregate is different. Among them, the high-performance concrete prepared in Example 8 has the best durability, tensile strength and deformation resistance.

[0070] Among Example 10, Example 11 and Example 3, the high performance concrete prepared in Example 3 has the best durability, tensile strength and deformation resistance.

[0071] Among Example 12, Example 13 and Example 3, the high performance concrete prepared in Example 3 has the best durability, tensile strength and deformation resistance.

[0072] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A high performance concrete, characterized in that: The raw material composition includes, by weight: 400-500 parts of cement, 120-300 parts of mineral admixture, 900-1000 parts of coarse aggregate, 600-750 parts of fine aggregate, 5-10 parts of polycarboxylic acid water reducer, 5-10 parts of modified polypropylene fiber, 120-150 parts of water, and 8-15 parts of polyethylene glycol-modified aliphatic epoxy resin.

2. The high performance concrete according to claim 1, characterized in that: The raw material composition includes, by weight: 420-480 parts of cement, 160-260 parts of mineral admixture, 920-980 parts of coarse aggregate, 650-700 parts of fine aggregate, 7-8 parts of polycarboxylic acid water-reducing agent, 7-8 parts of modified polypropylene fiber, 130-140 parts of water, and 10-13 parts of polyethylene glycol-modified aliphatic epoxy resin.

3. The high performance concrete according to claim 1, characterized in that: The mineral admixtures are fly ash and silica ash, and the weight ratio of the fly ash to the silica ash is 4-10:

1.

4. The high performance concrete according to claim 1, characterized in that: The coarse aggregate is 5~10mm and 16~25mm secondary grade crushed stone, and the mixing ratio is 1:2~3.

5. The high performance concrete according to claim 1, characterized in that: The fine aggregate is river sand, and the fineness modulus is 2.6-2.

9.

6. The high performance concrete according to claim 1, characterized in that: The preparation method of the modified polypropylene fiber is as follows: dispersing vinyl triethoxysilane in a solvent to obtain a vinyl triethoxysilane solution; immersing polypropylene fiber in the vinyl triethoxysilane solution for 30 to 60 minutes, and drying to obtain the modified polypropylene fiber.

7. The high performance concrete according to claim 6, characterized in that: The vinyl triethoxysilane accounts for 0.5-2wt% of the polypropylene fiber.

8. The high performance concrete according to claim 1, characterized in that: The polyethylene glycol-modified aliphatic epoxy resin is prepared by comprising polyethylene glycol and aliphatic epoxy resin, and the weight ratio of the polyethylene glycol to the aliphatic epoxy resin is 1:3-5.

9. The high performance concrete according to claim 8, characterized in that: The molecular weight of the aliphatic epoxy resin is 600-1000, and the epoxy equivalent of the aliphatic epoxy resin is 150-200 g / Eq.

10. A method for preparing high performance concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Mixing and stirring the coarse aggregate, fine aggregate, mineral admixture and modified polypropylene fiber in the formula amount to prepare a premix; S2, adding cement, polycarboxylate water-reducing agent, water, polyethylene glycol-modified aliphatic epoxy resin to the premix, mixing and stirring to obtain a concrete mixture; S3, injecting the concrete mixture into a mold for molding, curing, and demoulding to obtain the high performance concrete.

Citation Information

Patent Citations

  • High-performance premixed concrete and preparation method thereof

    CN113845344A

  • Steam-curing-free ultra-high performance concrete for bridge pier body and preparation method of steam-curing-free ultra-high performance concrete

    CN116283148A

  • High-temperature-resistant hot melt adhesive for PET bottle labeling and preparation process of high-temperature-resistant hot melt adhesive

    CN117447951A

  • Anti-cracking high-performance concrete and preparation method thereof

    CN117985981A

  • Reinforcing PVA fiber concrete composite and manufactuaring method thereof

    KR1020150142415A