Method for preparing oleophylic and hydrophobic TATB
By preparing low surface energy materials and treating TATB particles with metal salt solutions, the hygroscopicity problem of TATB was solved, improving its oleophilic and hydrophobic properties and making large-scale production feasible, making it suitable for TATB applications in military chemistry.
Patent Information
- Application Number
- CN202410951649.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
TATB is prone to moisture absorption during preparation, production, storage and application, which affects its performance. Existing technologies lack effective methods for moisture-proof modification.
The oleophilic and hydrophobic TATB is prepared by combining a low surface energy material solution and a metal salt solution with stirring and drying. The specific steps include adding TATB particles to the low surface energy material solution, stirring and filtering to dry, and then adding them to the metal salt solution, stirring and filtering to dry. Low surface energy materials such as decaoctanoic acid and perfluoropolyether are preferred, as well as metal salts such as copper nitrate and ferric acetate.
It significantly improves the oleophilic and hydrophobic properties of TATB, with a water contact angle ≥109° and a contact angle of 0° with common binders. The modification method is simple, the production cycle is short, and the cost is low. It is suitable for large-scale production and does not affect the detonation performance.
Smart Images

Figure CN118908789A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of anti-hygroscopicity of energetic materials, and more specifically, the present invention relates to a method for preparing oleophilic and hydrophobic TATB. Background Art
[0002] The study of high-energy insensitive materials is an important field of military chemistry in the world. 1,3,5-Triamino-2,4,6-trinitrobenzene (TATB) is a typical insensitive explosive with high crystal density, good thermal stability, and insensitivity to mechanical stimulation. It is one of the most important insensitive high-energy explosives at present. However, it is easy to absorb moisture during the preparation, production, storage, and application processes, which in turn affects its performance. Therefore, TATB needs to be modified before application to reduce its hygroscopicity so that it can be more widely used in modern military. However, there is little research on the anti-hygroscopicity of TATB at home and abroad.
[0003] The wettability of a solid surface is determined by its surface chemical composition and roughness. Low surface free energy and appropriate roughness are important factors in preparing superhydrophobic surfaces. The lower the surface free energy of a material, the stronger its hydrophobicity. Studying how to prepare an oleophilic and hydrophobic coating on the surface of TATB to improve its hygroscopicity is of great significance to the application of TATB in military chemistry and also provides a reference for the modification of other energetic materials. Summary of the invention
[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0005] In order to achieve these objects and other advantages of the present invention, a method for preparing lipophilic and hydrophobic TATB is provided, comprising the following steps:
[0006] Step 1, preparing a low surface energy material solution and a metal salt solution;
[0007] Step 2: adding TATB particles into a low surface energy material solution, stirring at a certain temperature and speed, filtering and drying, and obtaining preliminarily modified TATB particles;
[0008] Step 3: Add the preliminarily modified TATB particles obtained in step 1 to the metal salt solution, stir at a certain temperature and rotation speed, filter and dry to obtain lipophilic and hydrophobic TATB.
[0009] Preferably, in step 1, the low surface energy material is one or more of docosanoic acid, potassium docosanoate, sodium docosanoate, vinyl trimethoxysilane, vinyl triethoxysilane, 3-aminopropyl triethoxysilane, propyl triethoxysilane, γ-aminopropyl triethoxysilane, perfluoropolyether, and perfluorocarboxylic acid.
[0010] Preferably, in step 1, the metal salt is one or more of copper nitrate, copper chloride, copper sulfate, copper acetate, ferric nitrate, ferric chloride, ferric sulfate, ferric acetate, ferrous nitrate, ferrous chloride, ferrous sulfate, ferrous acetate, cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt acetate, copper nitrate, copper chloride, copper sulfate, copper acetate, zinc nitrate, zinc chloride, zinc sulfate, zinc acetate, nickel nitrate, nickel chloride, nickel sulfate, nickel acetate, silver nitrate, silver chloride, and silver acetate.
[0011] Preferably, in step 1, the solvent used for the low surface energy material solution is one or more of ethanol, n-butanol, isopropanol, ethyl acetate, butyl acetate, isoamyl acetate, acetic acid, propionic acid, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, ether, petroleum ether, n-butane, and cyclohexane.
[0012] Preferably, in step 1, the solvent used for the metal salt solution is one or more of ethanol, n-butanol, isopropanol, ethyl acetate, butyl acetate, isoamyl acetate, dichloromethane, chloroform, carbon tetrachloride, and ethylene dichloride.
[0013] Preferably, the mass volume ratio of the low surface energy material to the solvent in the low surface energy material solution is 0.002-0.03 g: 20-50 mL;
[0014] Preferably, the mass volume ratio of the metal salt to the solvent in the metal salt solution is 0.002-0.03 g:20-50 mL.
[0015] Preferably, in step 2, the mass of the low surface energy material is 0.01% to 5% of the mass of the TATB particles.
[0016] Preferably, in step three, the mass of the metal salt is 0.05% to 10% of the mass of the TATB particles.
[0017] Preferably, in step 2 and step 3, the stirring temperature is 20-80° C., the stirring speed is 100-500 r / min, and the stirring time is 0.5-3 h.
[0018] Preferably, the preparation method of the metal salt solution is: adding stearic acid to an ethanol aqueous solution, then adding zinc nitrate, copper nitrate and ferric nitrate, stirring at a certain temperature and speed, then adding gallic acid, stirring at a certain temperature and speed, performing electric field-ultrasonic field coupling treatment, vacuum drying to obtain a modified metal salt, taking the modified metal salt and adding it to ethanol to obtain a metal salt solution.
[0019] Preferably, the mass ratio of stearic acid, gallic acid and metal salt is 0.01-0.04:0.01-0.04:1; the concentration of ethanol aqueous solution is 40-80wt%; and the mass volume ratio of stearic acid and ethanol aqueous solution is 0.01-0.04g:100-300mL.
[0020] Preferably, the method of electric field-ultrasonic field coupling treatment is: placing the solution in a treatment chamber between two plates, the plate electrodes are copper electrodes, starting the power supply to generate a constant voltage electric field, the voltage is 1 to 5V; inserting an ultrasonic head into the solution, adjusting the ultrasonic output power to 100 to 300W, the frequency to 20 to 50kHz; and simultaneously turning on the electric field and ultrasonic treatment for 20 to 40 minutes.
[0021] The present invention at least includes the following beneficial effects: the present invention performs surface treatment on hygroscopic TATB particles, thereby improving the oleophilic and hydrophobic properties of TATB, with a water contact angle of ≥109°, and the contact angles with five common binder solutions of F2311, F2601, F2605, Esten, and HTPB are all 0°, which is very meaningful for the application of TATB in military chemistry and provides a new idea for preparing oleophilic and hydrophobic coatings of energetic materials; in addition, the method of the present invention is simple, has a short production cycle, high efficiency, high product quality and low cost, is suitable for large-scale production, and uses a small proportion of non-energetic materials, which will not affect the detonation performance of TATB.
[0022] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the water contact angle diagram of raw material TATB;
[0024] Figure 2 This is a water contact angle diagram of the lipophilic and hydrophobic TATB prepared in Example 1;
[0025] Figure 3 This is a SEM image of the lipophilic and hydrophobic TATB prepared in Example 1;
[0026] Figure 4 XRD diagrams of the lipophilic and hydrophobic TATB prepared in Example 1 and the raw material TATB;
[0027] Figure 5 FT-IR images of the lipophilic and hydrophobic TATB prepared in Example 1 and the raw material TATB;
[0028] Figure 6 This is a water contact angle diagram of the lipophilic and hydrophobic TATB prepared in Example 3;
[0029] Figure 7 The contact angle diagram of lipophilic and hydrophobic TATB and F2311 prepared in Example 5;
[0030] Figure 8 Contact angle diagram of raw material TATB and F2601. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0032] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0033] Example 1
[0034] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0035] Step 1: Add 0.025 g of 3-aminopropyltriethoxysilane to 30 mL of ethanol to obtain a low surface energy material solution; add 0.021 g of zinc nitrate to 30 mL of ethanol to obtain a metal salt solution;
[0036] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0037] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0038] The contact angle test was performed on the lipophilic and hydrophobic TATB prepared in this example. Figure 2 As shown, the contact angle of lipophilic and hydrophobic TATB with water is 146.1°, and the contact angles with ethyl acetate solutions of binders F2311, F2601, F2605, Esten, and HTPB (the mass volume ratio of binder to ethyl acetate is 0.01 g:5 mL, the same below) are all 0°.
[0039] Figure 3 This is a scanning electron microscope image of the lipophilic and hydrophobic TATB prepared in Example 1. Figure 4 The XRD diagrams of the lipophilic and hydrophobic TATB prepared in Example 1 and the raw material TATB are shown in FIG. Figure 5 The FT-IR images of the lipophilic and hydrophobic TATB prepared in Example 1 and the raw material TATB are shown. It can be seen that after the TATB is modified, the surface of the TATB is evenly coated, and its crystal form and thermal properties are not significantly changed.
[0040] Example 2
[0041] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0042] Step 1: Add 0.025 g of propyltriethoxysilane to 30 mL of ethanol to obtain a low surface energy material solution; add 0.019 g of copper sulfate to 30 mL of ethanol to obtain a metal salt solution;
[0043] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0044] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0045] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 143.6°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0046] Example 3
[0047] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0048] Step 1: Add 0.015 g of γ-aminopropyltriethoxysilane to 30 mL of ethyl acetate to obtain a low surface energy material solution; add 0.013 g of copper acetate to 30 mL of ethyl acetate to obtain a metal salt solution;
[0049] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0050] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0051] The contact angle test was performed on the lipophilic and hydrophobic TATB prepared in this example. Figure 6 As shown, its water contact angle is 138.7°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB are all 0°.
[0052] Example 4
[0053] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0054] Step 1: Add 0.015 g of stearic acid to 30 mL of ethyl acetate to obtain a low surface energy material solution; add 0.009 g of cobalt acetate to 30 mL of ethyl acetate to obtain a metal salt solution;
[0055] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0056] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0057] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 121.4°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0058] Example 5
[0059] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0060] Step 1: Add 0.005 g of perfluorocarboxylic acid to 30 mL of dichloromethane to obtain a low surface energy material solution; add 0.003 g of ferric nitrate to 30 mL of dichloromethane to obtain a metal salt solution;
[0061] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0062] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0063] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 109.9°. Its contact angles with the ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°. The contact angles of the lipophilic and hydrophobic TATB prepared in this example with the ethyl acetate solution of F2311 were as follows: Figure 7 shown.
[0064] Example 6
[0065] A method for preparing lipophilic and hydrophobic TATB comprises the following steps:
[0066] Step 1: Add 0.005 g of perfluoropolyether to 30 mL of dichloromethane to obtain a low surface energy material solution; add 0.003 g of manganese chloride to 30 mL of dichloromethane to obtain a metal salt solution;
[0067] Step 2: adding 0.5 g of TATB particles to the low surface energy material solution, stirring at 30° C. and 200 r / min for 0.5 h, filtering, and vacuum drying to obtain preliminarily modified TATB particles;
[0068] Step 3: Add the preliminarily modified TATB particles into the metal salt solution, stir at 30° C. and 300 r / min for 2 h, filter, and vacuum dry to obtain lipophilic and hydrophobic TATB.
[0069] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 113.4°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0070] like Figure 1 and Figure 8 As shown, the water contact angle of the raw material TATB is 0°, and the contact angle with the F2601 ethyl acetate solution is 0°. The water contact angles of the lipophilic and hydrophobic TATB prepared in Examples 1 to 6 are ≥109°, and the highest reaches 146.1° (Example 1), indicating that the method of the present invention can significantly improve the hydrophobicity of TATB.
[0071] Example 7
[0072] In the present embodiment, the preparation method of the metal salt solution is as follows: 0.02g of stearic acid is added to 200mL of 50wt% ethanol aqueous solution, 0.5g of zinc nitrate, 0.3g of copper nitrate and 0.2g of ferric nitrate are added, stirred at 30°C and 300r / min for 0.5h, 0.02g of gallic acid is added, stirred at 30°C and 300r / min for 0.5h, the obtained solution is placed in a treatment chamber between two copper electrode plates, a power supply is started to generate a constant voltage electric field, the voltage is 3V, an ultrasonic head is inserted into the solution, the ultrasonic output power is adjusted to 200W, the frequency is 30kHz, an electric field-ultrasonic field coupling treatment is performed for 30min, vacuum drying is performed to obtain a modified metal salt, 0.021g of the modified metal salt is added to 30mL of ethanol to obtain a metal salt solution. The remaining steps are the same as in Example 1.
[0073] In this embodiment, the metal salt is modified to improve the hydrophobicity and binding force of the metal salt, so that the metal salt can better adhere to the surface of TATB particles to form the rough structure required for the super-hydrophobic surface, thereby further improving the hydrophobicity of TATB. The contact angle test of the lipophilic and hydrophobic TATB prepared in this embodiment is performed, and its water contact angle is 156.7°, and its contact angle with the ethyl acetate solution of F2311, F2601, F2605, Esten, and HTPB is 0°.
[0074] Example 8
[0075] In this embodiment, the preparation method of the metal salt solution is as follows: 0.02g of stearic acid is added to 200mL of 50wt% ethanol aqueous solution, and then 0.5g of zinc nitrate, 0.3g of copper nitrate and 0.2g of ferric nitrate are added, and stirred at 30°C and 300r / min for 0.5h, and then 0.02g of gallic acid is added, and stirred at 30°C and 300r / min for 0.5h, and vacuum dried to obtain a modified metal salt, and 0.021g of the modified metal salt is added to 30mL of ethanol to obtain a metal salt solution. The remaining steps are the same as those in Example 1.
[0076] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 150.3°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0077] Example 9
[0078] In the present embodiment, the preparation method of the metal salt solution is as follows: 0.02g of stearic acid is added to 200mL of 50wt% ethanol aqueous solution, 0.5g of zinc nitrate, 0.3g of copper nitrate and 0.2g of ferric nitrate are added, stirred at 30°C and 300r / min for 0.5h, 0.02g of gallic acid is added, stirred at 30°C and 300r / min for 0.5h, an ultrasonic head is inserted into the obtained solution, the ultrasonic output power is adjusted to 200W, the frequency is 30kHz, ultrasonic treatment is performed for 30min, vacuum drying is performed to obtain a modified metal salt, 0.021g of the modified metal salt is added to 30mL of ethanol to obtain a metal salt solution. The remaining steps are the same as in Example 1.
[0079] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 152.8°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0080] Example 10
[0081] In this embodiment, the preparation method of the metal salt solution is as follows: 0.02g of stearic acid is added to 200mL of 50wt% ethanol aqueous solution, and then 0.5g of zinc nitrate, 0.3g of copper nitrate and 0.2g of ferric nitrate are added, and stirred at 30°C and 300r / min for 0.5h, and then 0.02g of gallic acid is added, and stirred at 30°C and 300r / min for 0.5h, and the obtained solution is placed in a treatment chamber between two copper electrode plates, and a power supply is started to generate a constant voltage electric field, and the voltage is 3V, and the electric field treatment is performed for 30min, and vacuum drying is performed to obtain a modified metal salt, and 0.021g of the modified metal salt is added to 30mL of ethanol to obtain a metal salt solution. The remaining steps are the same as those in Example 1.
[0082] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 153.0°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0083] Embodiment 11
[0084] In this embodiment, stearic acid is not added when preparing the metal salt solution, and the remaining steps are the same as those in Example 7.
[0085] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 154.6°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0086] Example 12
[0087] In this embodiment, gallic acid is not added when preparing the metal salt solution, and the remaining steps are the same as those in Example 7.
[0088] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 153.5°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0089] Example 13
[0090] In this embodiment, the preparation method of the metal salt solution is as follows: 0.5 g of zinc nitrate, 0.3 g of copper nitrate and 0.2 g of ferric nitrate are mixed evenly to obtain a mixed metal salt, and 0.021 g of the mixed metal salt is added to 30 mL of ethanol to obtain a metal salt solution. The remaining steps are the same as those in Example 1.
[0091] The contact angle test of the lipophilic and hydrophobic TATB prepared in this example showed that its water contact angle was 147.5°, and its contact angles with ethyl acetate solutions of F2311, F2601, F2605, Esten, and HTPB were all 0°.
[0092] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing lipophilic and hydrophobic TATB, It is characterized in that The following steps are involved: Step 1, preparing a low surface energy material solution and a metal salt solution; Step 2: adding TATB particles into a low surface energy material solution, stirring at a certain temperature and speed, filtering and drying, and obtaining preliminarily modified TATB particles; Step 3: Add the preliminarily modified TATB particles obtained in step 1 to the metal salt solution, stir at a certain temperature and rotation speed, filter and dry to obtain lipophilic and hydrophobic TATB.
2. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 1, It is characterized in that In the step 1, the low surface energy material is one or more of 1-pentadecosanoic acid, potassium 1-pentadecosanoate, sodium 1-pentadecosanoate, vinyl trimethoxysilane, vinyl triethoxysilane, 3-aminopropyl triethoxysilane, propyl triethoxysilane, γ-aminopropyl triethoxysilane, perfluoropolyether, and perfluorocarboxylic acid.
3. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 1, It is characterized in that In the step 1, the metal salt is one or more of copper nitrate, copper chloride, copper sulfate, copper acetate, ferric nitrate, ferric chloride, ferric sulfate, ferric acetate, ferrous nitrate, ferrous chloride, ferrous sulfate, ferrous acetate, cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt acetate, copper nitrate, copper chloride, copper sulfate, copper acetate, zinc nitrate, zinc chloride, zinc sulfate, zinc acetate, nickel nitrate, nickel chloride, nickel sulfate, nickel acetate, silver nitrate, silver chloride, and silver acetate.
4. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 2, It is characterized in that In the step 1, the solvent used for the low surface energy material solution is one or more of ethanol, n-butanol, isopropanol, ethyl acetate, butyl acetate, isoamyl acetate, acetic acid, propionic acid, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, ether, petroleum ether, n-butane, and cyclohexane.
5. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 3, It is characterized in that In the step 1, the solvent used for the metal salt solution is one or more of ethanol, n-butanol, isopropanol, ethyl acetate, butyl acetate, isoamyl acetate, dichloromethane, chloroform, carbon tetrachloride, and ethylene dichloride.
6. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 4, It is characterized in that The mass volume ratio of the low surface energy material to the solvent in the low surface energy material solution is 0.002-0.03 g: 20-50 mL.
7. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 5, It is characterized in that The mass volume ratio of the metal salt to the solvent in the metal salt solution is 0.002-0.03 g:20-50 mL.
8. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 1, It is characterized in that In the step 2, the mass of the low surface energy material is 0.01% to 5% of the mass of the TATB particles.
9. A method for preparing lipophilic and hydrophobic TATB as claimed in claim 1, It is characterized in that In the step 3, the mass of the metal salt is 0.05% to 10% of the mass of the TATB particles.
10. A method for preparing lipophilic and hydrophobic TATB according to claim 1, It is characterized in that In the step 2 and step 3, the stirring temperature is 20-80° C., the stirring speed is 100-500 r / min, and the stirring time is 0.5-3 h.
Citation Information
Patent Citations
Ultra hydrophobic surface preparation method
CN101417278A
Conductive polymer composite with super hydrophobicity and preparation method thereof
CN101798461A
Multifunctional superhydrophobic particles for chemical adhesion and blooming
CN107250291A
Method for preparing superhydrophobic oxidant based on lotus effect
CN109206284A
Method of fabricating surface body having superhydrophobicity and hydrophilicity and apparatus of preparing the same
US20140322455A1