Composite solid propellant and rapid curing forming method thereof
By using graphene composite aluminum powder in composite solid propellant to accelerate the thermal curing reaction of the adhesive, the problem of long curing time of composite solid propellant is solved, and the production efficiency is improved and the combustion performance is maintained.
Patent Information
- Application Number
- CN202411008691.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Existing composite solid propellants take a long time to fully heat cure at temperatures that meet production safety, resulting in low production efficiency.
Graphene composite aluminum powder is used as metal fuel, and the aluminum particles are modified with fluoride and graphene dispersion to form a highly thermally conductive graphene composite aluminum powder, and introduced it into the composite solid propellant, and is vacuum drying and heat curing. Technology shortens curing and forming time.
The curing and forming time of composite solid propellant is shortened, from 7 to 8 days to 5 to 6 days, improving production efficiency while maintaining combustion performance and energy levels.
Smart Images

Figure BDA0004963682610000051 
Figure HDA0004963682620000011 
Figure HDA0004963682620000012
Abstract
Description
Technical Field
[0001] The invention relates to a rapid solidification molding method for a composite solid propellant, belonging to the technical field of composite materials. Background Art
[0002] Composite solid propellant, as an energetic composite material, is the power source of various solid rocket engines. Its performance directly determines the combat effectiveness and survivability of missile weapons and spacecraft. Therefore, solid propellant plays an important role in the development of missile and aerospace technology.
[0003] Composite solid propellants are mainly composed of polymer prepolymers, inorganic oxides (such as ammonium perchlorate), metal fuels (aluminum powder) and other functional additives. Among them, the polymer prepolymer binds all solid phases together, forms a three-dimensional network through chemical cross-linking reactions, and then solidifies under thermal conditions to form an elastic composite solid propellant. Therefore, the curing of the binder system is the basis for the solid propellant to have excellent combustion performance, mechanical properties, structural integrity and effective storage of huge chemical energy.
[0004] In order to control the optimal curing process, curing temperature and curing time are two key parameters that can determine the curing cross-linking reaction as well as mechanical and combustion properties. The higher the temperature, the faster the curing reaction and the higher the production efficiency, but there are also safety hazards such as explosion. Existing composite solid propellants often take a long time to fully heat cure at a temperature that meets production safety, and the production efficiency is relatively low. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a composite solid propellant and a rapid curing molding method thereof in view of the deficiencies in the above-mentioned prior art, thereby shortening the curing molding time of the composite solid propellant and improving the production efficiency.
[0006] The technical solution adopted by the present invention to solve the above-mentioned problems is:
[0007] A composite solid propellant, whose raw material composition includes an oxidant, a metal fuel and an adhesive, a plasticizer and a curing agent, characterized in that: the metal fuel adopts one or two of aluminum powder and graphene composite aluminum powder, and must contain graphene composite aluminum powder; the total amount of metal fuel accounts for 15-20% of the mass percentage of the composite solid propellant, wherein the mass percentage of graphene in the composite solid propellant is not less than 0.18%, and preferably the mass percentage of graphene in the composite solid propellant is 0.18%-0.75%.
[0008] Furthermore, the raw material composition of the composite solid propellant comprises, by mass percentage, 65-70% oxidizer, 15-20% metal fuel, 8-14% binder, 2-3% plasticizer, and 0.75-1.25% curing agent.
[0009] According to the above scheme, the oxidant is preferably ammonium perchlorate (AP) or the like, the adhesive is preferably terminal hydroxyl polybutadiene (HTPB) or the like; the curing agent is preferably isophorone diisocyanate (IPDI) or the like; the plasticizer is preferably dioctyl sebacate (DOS) or the like.
[0010] According to the above scheme, the graphene composite aluminum powder is a spherical composite of graphene composited on the surface of aluminum particles, wherein the aluminum particles are pre-modified with fluoride.
[0011] Furthermore, the present invention provides a method for preparing the above-mentioned graphene composite aluminum powder, comprising the following steps:
[0012] (1) dissolving a fluoride in an organic solvent, then adding the fluoride to a dispersion of spherical aluminum particle powder, mixing and stirring the mixture evenly, separating a solid product, and obtaining fluoride-modified spherical aluminum particles; wherein the mass percentage of the fluoride relative to the aluminum particles is 8 to 12%;
[0013] (2) dispersing the graphene in a solvent by ultrasonic treatment to obtain a graphene dispersion;
[0014] (3) adding the fluoride-modified spherical aluminum particles obtained in step (1) to the graphene dispersion of step (2), wherein the mass percentage of graphene relative to the aluminum particles before fluoride modification is 3 to 8%, mixing and stirring uniformly, and then separating the solid product to obtain a spherical composite of graphene dispersed on the surface of the aluminum particles (i.e., graphene composite aluminum powder, the mass percentage of graphene in the graphene composite aluminum powder is 2.9 to 7.4%).
[0015] According to the above scheme, in step (1), the fluoride is polyvinylidene fluoride (PVDF), and its organic solvent is preferably N,N-dimethylformamide (DMF), and the mass concentration of the fluoride dissolved in the organic solvent is 3-5 mg / ml.
[0016] According to the above scheme, in step (1), the particle size distribution D of the spherical aluminum particles is 50 4~5μm.
[0017] According to the above scheme, the dispersion liquid of the aluminum particle powder adopts a mixed solvent of water and ethanol, and the mass concentration of the dispersion liquid is preferably 20-30 mg / ml, and the volume ratio of the mixed solvent preferably is 1:1 between water and ethanol.
[0018] According to the above scheme, the graphene dispersion liquid adopts a mixed solvent of water and ethanol, and the mass concentration of graphene is preferably 0.4-0.6 mg / ml. Further, the mixed solvent adopted by the graphene dispersion liquid preferably has a volume ratio of water to ethanol of 10:1.
[0019] According to the above scheme, the graphene containing sulfonated groups is prepared from sulfonated polyetheretherketone and graphene as raw materials. The specific preparation method is: adding flaky graphene oxide GO to the aqueous solution of the macromolecular polymer sulfonated polyetheretherketone SPEEK, and performing ultrasonic dispersion treatment, grafting the sulfonated groups to the graphene oxide through non-covalent interaction, and then reducing it with hydrazine hydrate, and finally vacuum freeze-drying to obtain fluffy graphene containing sulfonated groups. Among them, the mass ratio between graphene oxide GO and polymer sulfonated polyetheretherketone SPEEK is preferably (8-12): 1, and the concentration of the polymer sulfonated polyetheretherketone SPEEK aqueous solution is preferably 0.1-0.2 mg / ml; the time of ultrasonic dispersion treatment is preferably 40-60 min; the mass ratio of GO and hydrazine hydrate is preferably 1:1; the temperature of the reduction reaction is 90-110°C, and the time of the reduction reaction is 5-6 hours.
[0020] In a second aspect, the present invention further provides a method for rapid solidification molding of the composite solid propellant, comprising the following steps:
[0021] 1) Stirring and mixing the binder and the plasticizer evenly, dropping the curing agent, and continuing to stir and mix evenly; then adding the graphene composite aluminum powder and stirring and mixing evenly, and then adding the oxidant ammonium perchlorate and further stirring and mixing evenly, so as to obtain a composite solid propellant slurry; wherein the stirring and mixing time for each time is preferably 15 to 20 minutes;
[0022] 2) The composite solid propellant slurry is poured into a mold to be shaped, and is placed in a vacuum drying oven at 50 to 60° C. and -0.08 MPa for degassing, and then placed in an oven at 60 to 70° C. for thermal curing to obtain a composite solid propellant.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The composite solid propellant of the present invention not only has the advantages of high combustion energy release efficiency, good thermal conductivity, and excellent overall combustion performance, but also shortens the curing time of the composite solid propellant to a certain extent, thereby improving production efficiency. Specifically:
[0025] 1) The present invention obtains graphene composite aluminum powder by introducing high thermal conductivity graphene (specifically sulfonated graphene) into PVDF-modified spherical aluminum particles, and then uses the composite structure of the graphene composite aluminum powder to uniformly introduce the high thermal conductivity graphene into the adhesive matrix of the composite solid propellant (the adhesive matrix here refers to the adhesive and the plasticizer and the curing agent), thereby obtaining a composite solid propellant slurry with high internal thermal conductivity, which can effectively accelerate the thermal curing reaction of the adhesive matrix, shorten the curing molding time of the composite solid propellant to a certain extent, and improve the production efficiency.
[0026] 2) The existing composite solid propellant charge curing molding technology generally requires 7 to 8 days to be completely cured in a 60°C thermal environment; however, the thermal curing molding time of the composite solid propellant of the present invention can be reduced from the original 7 to 8 days to 5 to 6 days after being accelerated by the graphene composite aluminum powder.
[0027] 3) The preparation process of the composite solid propellant of the present invention is simple, the raw materials are easily available, the required cost is low, and the energy level and combustion performance of the prepared composite solid propellant only increase and not decrease. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the SEM image of graphene composite aluminum powder Al / PVDF / Gr.
[0029] Figure 2 This is a SEM-EDS image of the cross section of the composite solid propellant of Example 1.
[0030] Figure 3 The figure is a comparison chart of the burning speed of the composite solid propellant of Example 1 and the comparative example.
[0031] Figure 4 This is a SEM comparison image of the combustion products of the composite solid propellant of Example 1.
[0032] Figure 5 This is the curing process curve of Example 1.
[0033] Figure 6 This is the curing process curve of Example 2.
[0034] Figure 7 This is the curing process curve of Example 3.
[0035] Figure 8 This is the curing molding process curve of Example 4.
[0036] Fig. 9 This is the curing process curve of the comparative example. DETAILED DESCRIPTION
[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0038] In the following embodiments, the preparation method of the graphene composite aluminum powder adopted comprises the following specific steps:
[0039] (1) 1 g of spherical aluminum particle powder with a particle size of 4 to 5 μm was selected, and the mixture was dispersed in a mixed solvent of 20 ml of deionized water and 20 ml of ethanol to obtain a dispersion of the aluminum particle powder; a PVDF solution (prepared from 80 mg of PVDF and 20 ml of DMF) was gradually added to the dispersion of the aluminum particle powder at a flow rate of 2 ml / min, and after stirring for 1 hour, the mixture was filtered and dried to obtain a fluoride-modified spherical aluminum particle powder (abbreviated as Al / PVDF powder);
[0040] (2) Weighing 50 mg of sulfonated graphene, and ultrasonically dispersing it in a mixed solvent of 100 ml of deionized water and 10 ml of ethanol to obtain a graphene dispersion;
[0041] (3) Add Al / PVDF powder to the above graphene (Gr) dispersion, stir for 1 h, and dry to obtain graphene composite aluminum powder, abbreviated as Al / PVDF / Gr powder, such as Figure 1 As shown, the surface of the aluminum powder is combined with granular PVDF and flake sulfonated graphene. In terms of mass percentage, the Al / PVDF / Gr powder has an Al content of 88.5wt%, a PVDF content of 7.1wt%, and a Gr content of 4.4wt%.
[0042] In the preparation method of the above-mentioned graphene composite aluminum powder, by adjusting the amount of graphene added relative to aluminum powder, graphene composite aluminum powder with different graphene contents can be obtained. The mass percentage of graphene in the graphene composite aluminum powder is 2.9-7.4%, which can all be used in the present invention, and the mass percentage of graphene in the composite solid propellant is controlled to be not less than 0.18%.
[0043] In the preparation method of the above-mentioned graphene composite aluminum powder, sulfonated graphene is obtained through the following preparation process: 100 mg of flaky graphene oxide GO (1-5 μm diameter, 1-2 layers) is added to 100 ml of 0.1 mg / ml macromolecular polymer sulfonated polyetheretherketone SPEEK aqueous solution, and ultrasonic dispersion treatment is performed for 1 hour, and the sulfonated group is grafted to the graphene oxide through non-covalent interaction, and then 0.1 ml of 80% hydrazine hydrate is taken for reduction, and the reaction is placed at a temperature of 100° C. for 5-6 hours, and then vacuum freeze-drying treatment is performed to obtain fluffy graphene containing sulfonated groups.
[0044] In the following embodiments, the indentation size is tested by a Wilson Tukon 1202 digital microhardness tester to determine the molding process of the composite solid propellant. The loading pressure is 25 g. The indentation size of each sample is tested every 12 hours, and each sample is tested 3 times at different positions without interfering with each other. The average indentation size obtained is the test result. After the test, a solidification molding process curve is plotted with the indentation size as the ordinate and the time as the abscissa.
[0045] In the following examples, the composite solid propellant was cut into 5 mm × 5 mm × 10 mm strips, and the combustion rate of the composite solid propellant under different pressures (0.5 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa) in a nitrogen atmosphere was tested by a high-pressure laser ignition combustion test system, and the combustion products were collected. After the test, the pressure was used as the abscissa and the combustion rate was used as the ordinate to mark the combustion rate of the propellant, and a straight line was fitted. According to the Vieille formula r = ap n The burning rate-pressure relationship was obtained.
[0046] In the following embodiments, the oxidant is ammonium perchlorate (AP), which is a white crystal; the adhesive is hydroxy-terminated polybutadiene, which is a colorless or light yellow transparent liquid; the plasticizer is dioctyl sebacate (DOS), which is a colorless or light yellow oily liquid; and the curing agent is isophorone diisocyanate (IPDI), which is a colorless to slightly yellow liquid.
[0047] Example 1
[0048] A composite solid propellant, wherein the raw material composition system is calculated by mass percentage as follows: AP 68%, Al / PVDF / Gr powder 17% (the graphene in the Al / PVDF / Gr powder accounts for about 0.75% of the mass percentage of the composite solid propellant), adhesive HTPB 12%, plasticizer DOS 2%, and curing agent IPDI 1%. The preparation method thereof comprises the following steps:
[0049] 1) 2.4 g of adhesive HTPB was placed in a container, 0.4 g of plasticizer DOS was added dropwise, and the mixture was stirred for 15 min to be evenly mixed, and 0.2 g of curing agent IPDI was added dropwise and stirred for 15 min to be evenly mixed to obtain an adhesive matrix; 3.4 g of graphene composite aluminum powder Al / PVDF / Gr was added to the adhesive matrix, and the mixture was evenly mixed for 15 min, and then 13.6 g of ammonium perchlorate AP was added and evenly mixed for 15 min, so that all solid components were fully coated and wetted by the adhesive matrix to obtain a high-viscosity composite solid propellant slurry;
[0050] 2) Thermal curing molding: The composite solid propellant slurry is poured into a PTFE mold, placed in a vacuum drying oven at 50°C and -0.08MPa to remove bubbles for 12 hours, and then placed in an oven at 60°C for curing to obtain a cured composite solid propellant.
[0051] Depend on Figure 2 It can be seen that the cross-sectional structure of the composite solid propellant is complete, the oxide AP, composite aluminum powder, and binder matrix are evenly distributed, and its energy spectrum characterization of Al, F, and S elements shows that the structure of the composite aluminum powder in the composite aluminum powder propellant is still intact.
[0052] The composite solid propellant prepared in Example 1 was cut into 5 mm × 5 mm × 10 mm strips. The combustion speed of the composite solid propellant under different pressures (0.5 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa) in a nitrogen atmosphere was tested by a high-speed photography laser ignition combustion test system and the combustion products were collected. After the test, the propellant combustion speed was marked with pressure as the abscissa and the combustion speed as the ordinate, and a straight line was fitted. According to the Vieille formula r = a p n The burning rate-pressure relationship was obtained. Figure 3 Table 1 is a comparison chart of the burning speed of the composite solid propellant of Example 1 and the comparative example. Figure 3 Specific burning rate values, wherein ACSP-1 represents a comparative example; ACSP-2 represents Example 1.
[0053] Table 1
[0054]
[0055] Depend on Figure 3 As shown in Table 1, the burning speed of the composite solid propellant of Example 1 is faster; Figure 4 It can be seen that the combustion products of the composite solid propellant of Example 1 have no obvious agglomeration and are sparsely dispersed, indicating that its combustion efficiency is higher.
[0056] Depend on Figure 5 It can be seen that the molding time of the composite solid propellant obtained in Example 1 is about 132 hours, about 5.5 days.
[0057] Example 2
[0058] A composite solid propellant, the raw material composition of which is calculated by mass percentage: AP 68%, Al / PVDF / Gr powder 12.75% (the graphene in the Al / PVDF / Gr powder accounts for about 0.55% of the mass percentage of the composite solid propellant), aluminum powder (spherical aluminum particle powder of 4-5 μm) 4.25%, binder HTPB 12%, plasticizer DOS 2%, curing agent IPDI 1%, and the preparation method thereof comprises the following steps:
[0059] 1) 2.4 g of adhesive HTPB was placed in a container, 0.4 g of plasticizer DOS was added dropwise, and the mixture was stirred for 15 min to be evenly mixed, and 0.2 g of curing agent IPDI was added dropwise and stirred for 15 min to be evenly mixed to obtain an adhesive matrix; 2.55 g of graphene composite aluminum powder Al / PVDF / Gr and 0.85 g of aluminum powder were added to the adhesive matrix, and the mixture was evenly mixed for 15 min, and 13.6 g of ammonium perchlorate AP was added and evenly mixed for 15 min, so that all solid components were fully coated and wetted by the adhesive matrix to obtain a high-viscosity composite solid propellant slurry;
[0060] 2) Thermal curing molding: The composite solid propellant slurry is poured into a PTFE mold, placed in a vacuum drying oven at 50°C and -0.08MPa to remove bubbles for 12 hours, and then placed in an oven at 60°C for curing to obtain a cured composite solid propellant.
[0061] Depend on Figure 6 It can be seen that the molding time of the composite solid propellant obtained in Example 2 is about 156 hours.
[0062] Example 3
[0063] A composite solid propellant, wherein the raw material composition system is calculated by mass percentage as follows: AP 68%, Al / PVDF / Gr powder 8.5% (the graphene in the Al / PVDF / Gr powder accounts for about 0.37% of the mass percentage of the composite solid propellant), aluminum powder (spherical aluminum particle powder of 4-5 μm) 8.5%, binder HTPB 12%, plasticizer DOS 2%, curing agent IPDI 1%, and the preparation method thereof comprises the following steps:
[0064] 1) 2.4 g of binder HTPB was placed in a container, 0.4 g of plasticizer DOS was added dropwise, and the mixture was stirred for 15 min to be evenly mixed, and 0.2 g of curing agent IPDI was added dropwise and stirred for 15 min to be evenly mixed, to obtain a binder matrix; 1.7 g of graphene composite aluminum powder Al / PVDF / Gr and 1.7 g of aluminum powder were added to the binder matrix, and the mixture was evenly mixed for 15 min, and 13.6 g of ammonium perchlorate AP was added and evenly mixed for 15 min to obtain a high-viscosity composite solid propellant slurry in which all solid components were fully coated and wetted by the binder system;
[0065] 2) Thermal curing molding: The composite solid propellant slurry is poured into a PTFE mold, placed in a vacuum drying oven at 50°C and -0.08MPa to remove bubbles for 12 hours, and then placed in an oven at 60°C for curing to obtain a cured composite solid propellant.
[0066] Depend on Figure 7It can be seen that the molding time of the composite solid propellant obtained in Example 3 is about 168h.
[0067] Example 4
[0068] A composite solid propellant, wherein the raw material composition system is calculated by mass percentage as follows: AP 68%, Al / PVDF / Gr powder 4.25% (the graphene in the Al / PVDF / Gr powder accounts for about 0.19% of the mass percentage of the composite solid propellant), aluminum powder (spherical aluminum particle powder of 4-5 μm) 12.75%, binder HTPB 12%, plasticizer DOS 2%, curing agent IPDI 1%, and the preparation method thereof comprises the following steps:
[0069] 1) 2.4 g of adhesive HTPB was placed in a container, 0.4 g of plasticizer DOS was added dropwise, and the mixture was stirred for 15 min to be evenly mixed, and 0.2 g of curing agent IPDI was added dropwise and stirred for 15 min to be evenly mixed to obtain an adhesive matrix; 0.85 g of graphene composite aluminum powder Al / PVDF / Gr and 2.55 g of aluminum powder were added to the adhesive matrix, and the mixture was mixed evenly for 15 min, and 13.6 g of ammonium perchlorate AP was added and mixed evenly for 15 min to obtain a high-viscosity composite solid propellant slurry in which all solid components were fully coated and wetted by the adhesive system;
[0070] 2) Thermal curing molding: The composite solid propellant slurry is poured into a PTFE mold, placed in a vacuum drying oven at 50°C and -0.08MPa to remove bubbles for 12 hours, and then placed in an oven at 60°C for curing to obtain a cured composite solid propellant.
[0071] Depend on Figure 8 It can be seen that the molding time of the composite solid propellant obtained in Example 4 is about 168h.
[0072] Comparative Example
[0073] A composite solid propellant, the raw material composition system of which is calculated by mass percentage as follows: AP 68%, Al powder (spherical aluminum particle powder of 4-5 μm) 17%, binder HTPB 12%, plasticizer DOS 2%, curing agent IPDI 1%, and the preparation method thereof comprises the following steps:
[0074] 1) 2.4 g of binder HTPB was placed in a container, 0.4 g of plasticizer DOS was added dropwise, and the mixture was stirred for 15 min to be evenly mixed, and 0.2 g of curing agent IPDI was added dropwise and stirred for 15 min to be evenly mixed to obtain a binder matrix; 3.4 g of Al powder was added to the binder matrix, and the mixture was evenly mixed for 15 min, and 13.6 g of ammonium perchlorate AP was added and evenly mixed for 15 min to obtain a high-viscosity composite solid propellant slurry in which all solid components were fully coated and wetted by the binder system;
[0075] 2) Thermal curing molding: The composite solid propellant slurry is poured into a PTFE mold, placed in a vacuum drying oven at 50°C and -0.08MPa to remove bubbles for 12 hours, and then placed in an oven at 60°C for curing to obtain a cured composite solid propellant.
[0076] Depend on Fig. 9 It can be seen that the molding time of the composite solid propellant obtained in the comparative example is about 180h.
[0077] In summary, according to the composite solid propellants of Examples 1 to 4 and the comparative example, after the high thermal conductivity graphene is uniformly introduced into the composite solid propellant in the form of graphene composite aluminum powder microspheres, the curing process is accelerated to a certain extent, and according to the metal fuel used in Examples 1 to 4, as the amount of Al / PVDF / Gr powder increases and the amount of aluminum powder decreases, the curing molding speed of the composite solid propellant becomes faster and faster.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A composite solid propellant, the raw material composition includes an oxidizer, a metal fuel and a binder, a plasticizer and a curing agent, characterized in that: The metal fuel uses one or two of aluminum powder and graphene composite aluminum powder, and must contain graphene composite aluminum powder; the total amount of metal fuel accounts for 15-20% of the mass percentage of the composite solid propellant, wherein the mass percentage of graphene in the composite solid propellant is not less than 0.18%; the graphene composite aluminum powder is a spherical composite of graphene composited on the surface of fluoride-modified aluminum particles.
2. A composite solid propellant according to claim 1, characterized in that: The raw material composition includes, by mass percentage, 65-70% of oxidant, 15-20% of metal fuel, 8-14% of adhesive, 2-3% of plasticizer, and 0.75-1.25% of curing agent.
3. A composite solid propellant according to claim 1, characterized in that: The oxidant is ammonium perchlorate, the adhesive is terminal hydroxyl polybutadiene, the curing agent is isophorone diisocyanate, and the plasticizer is dioctyl sebacate.
4. A composite solid propellant according to claim 1, characterized in that: The method for preparing the graphene composite aluminum powder comprises the following steps: (1) dissolving a fluoride in an organic solvent, then adding the fluoride to a dispersion of spherical aluminum particle powder, mixing and stirring the mixture evenly, separating a solid product, and obtaining fluoride-modified spherical aluminum particles; wherein the mass percentage of the fluoride relative to the aluminum particles is 8 to 12%; (2) dispersing the graphene in a solvent by ultrasonic treatment to obtain a graphene dispersion; (3) adding the fluoride-modified spherical aluminum particles obtained in step (1) to the graphene dispersion in step (2), mixing and stirring evenly, and separating out a solid product, namely, graphene composite aluminum powder, which is a spherical composite in which graphene is dispersed on the surface of aluminum particles.
5. A composite solid propellant according to claim 4, characterized in that: In step (1), the fluoride is polyvinylidene fluoride, which is dissolved in an organic solvent, N,N-dimethylformamide, with a mass concentration of 3 to 5 mg / ml.
6. A composite solid propellant according to claim 4, characterized in that: In step (1), in step (1), the particle size distribution D of the spherical aluminum particles is 50 The aluminum particle powder dispersion adopts a mixed solvent of water and ethanol, and the preferred mass concentration of the dispersion is 20 to 30 mg / ml.
7. A composite solid propellant according to claim 4, characterized in that: The graphene dispersion liquid adopts a mixed solvent of water and ethanol, and the amount of graphene used is 5-8% of the mass of the spherical aluminum particles.
8. A composite solid propellant according to claim 4, characterized in that: The graphene is graphene containing sulfonated groups, and is prepared from sulfonated polyetheretherketone and graphene as raw materials. The specific preparation method is: adding flaky graphene oxide to a sulfonated polyetheretherketone aqueous solution, and performing ultrasonic dispersion treatment, grafting the sulfonated groups to the graphene oxide through non-covalent interaction, and then reducing with hydrazine hydrate, and finally performing vacuum freeze-drying treatment to obtain the graphene containing sulfonated groups.
9. The rapid solidification molding method of composite solid propellant according to claim 1, characterized in that: The following steps are involved: 1) Stir and mix the binder and plasticizer evenly, drop the curing agent, and continue to stir and mix evenly; then add the metal fuel and stir and mix evenly, and then add the oxidant and stir and mix evenly to obtain a composite solid propellant slurry; 2) The composite solid propellant slurry is cast and shaped, and after degassing in a vacuum environment of 50 to 60° C., it is placed in a temperature of 60 to 70° C. for thermal curing to obtain a composite solid propellant.
10. The rapid solidification molding method of composite solid propellant according to claim 9, characterized in that: In step 1), each stirring and mixing time is 15 to 20 minutes.
Citation Information
Patent Citations
Composite solid propellant and preparation method thereof
CN105801327A
Graphene-metal or semimetal shell-core structure composite material and preparation method thereof
CN106045794A
Al / CuO / porous graphene nano-composite energetic material and preparation method thereof
CN107353171A
Coaxial 3D printing method for improving burning speed of solid propellant and propellant
CN118108555A
IN3857DE2011A