Fluorine sulfonyl carboxylic ester, preparation method thereof, electrolyte and battery
By using fluorosulfonyl carboxylate as an additive in lithium-ion batteries to form a protective film, the problem of electrolyte instability under high voltage is solved, and the battery's high voltage resistance and low temperature performance are improved.
Patent Information
- Application Number
- CN202410935049.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
AI Technical Summary
When existing lithium-ion batteries are used at high voltages, the traditional electrolyte is unstable, which leads to an increase in side reactions and affects the battery's high voltage and low temperature performance.
By using fluorosulfonyl carboxylic acid esters as additives, the high-voltage resistance of the battery is improved by forming a dense protective film of lithium fluoride and an organic protective film, and the low-temperature performance is improved by regulating the length of the carboxylic acid ester chain segments in the molecular structure.
It improves the battery's high-voltage resistance and cycle performance, while also taking into account low-temperature performance, thus avoiding the negative impact of increased electrolyte viscosity on battery performance.
Smart Images

Figure CN118908863A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrolytes, and in particular relates to a fluorosulfonyl carboxylate and a preparation method thereof, an electrolyte and a battery. Background Art
[0002] As the application scope of lithium-ion batteries becomes wider and wider, battery life and operating temperature conditions have become the key to competition among various battery companies. Increasing the upper voltage limit of the battery is an effective way to improve the mass-to-energy ratio of the battery, but with the increase in voltage, traditional electrolytes will no longer be suitable for high-voltage systems. In traditional electrolyte systems, vinylene carbonate is the most commonly used electrolyte additive, which can form a film on the surface of the negative electrode and extend the overall cycle stability of the battery.
[0003] However, in high-voltage systems, vinylene carbonate is unstable and easily oxidized under high-voltage conditions, resulting in side reactions that cause battery failure.
[0004] To address the defect of vinyl carbonate's high-voltage instability, a common method is to use fluorinated additives to improve the high-voltage resistance of the electrolyte. Commonly used fluorinated additives include fluorinated vinyl carbonate, etc. This fluorinated additive can improve the battery surface interface and form a thin and dense interface protection film during formation, thereby improving the overall voltage resistance of the battery.
[0005] At the same time, in order to improve the battery cycle performance under high voltage, sulfur-containing additives such as vinyl sulfate, 1,3-propane sultone, etc. are usually used. Sulfur-containing additives can effectively prevent the side reactions of solvents such as vinyl carbonate and ethyl methyl carbonate under high voltage, thereby improving the overall cycle performance of the battery.
[0006] However, the addition of fluorinated additives and sulfur-containing additives will also bring certain disadvantages, especially the low-temperature performance of the battery. The addition of fluorinated additives will significantly increase the overall viscosity of the electrolyte, seriously hindering the diffusion of the electrolyte inside the electrode. The addition of sulfur-containing additives will form a high-impedance interface protection film, which will also affect the low-temperature performance of the battery.
[0007] In order to improve the low-temperature performance of batteries, carboxylic acid esters have become the mainstream solvents for low-temperature electrolytes. Carboxylic acid esters can change the viscosity of electrolytes and improve the low-temperature performance of batteries. Using carboxylic acid esters to improve the overall fluidity of additives and improve the overall electrical properties of fluorine-containing and sulfur-containing additives is an important direction at present. Summary of the invention
[0008] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a fluorosulfonyl carboxylate and a preparation method thereof, an electrolyte and a battery.
[0009] To achieve the above object, the technical solution adopted by the present invention is:
[0010] A fluorosulfonyl carboxylate, characterized in that it has a structure of formula (I);
[0011]
[0012] Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4.
[0013] Preferably, the R1 is selected from a molecular chain segment with 1-3 carbon atoms, and the value of n is 1-3; preferably, the R1 is methyl, ethyl, isopropyl; preferably, n is 1.
[0014] Preferably, the fluorosulfonyl carboxylate may be one of formulas (A1), (A2), (A3), and (A4).
[0015]
[0016]
[0017] The present invention also includes a method for preparing the fluorosulfonyl carboxylate, as shown in formula (II):
[0018]
[0019] Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4.
[0020] Specifically, the method comprises the following steps: under cooling conditions, gradually adding tetrafluoroethane-β-sultone to the R1-nOH alcohol substance; after the addition is completed, gradually returning the temperature to room temperature for reaction, and obtaining the product after treatment.
[0021] The molar ratio of tetrafluoroethane-β-sultone to the alcoholic hydroxyl group in the R1-nOH alcohol substance is 1:(1-1.2).
[0022] The specific treatment process is to blow away the residual hydrofluoric acid with nitrogen, wash the reaction mixture with water and brine, and collect the organic phase; then dry, filter and distill to obtain the final product.
[0023] The present invention also includes an electrolyte, comprising the fluorosulfonyl carboxylate, a solvent, a lithium salt and an additive. Preferably, the solvent accounts for 80-95 parts by weight, the lithium salt accounts for 12-15 parts by weight, the fluorosulfonyl carboxylate accounts for 0.5-6 parts by weight, and the additive accounts for 1.5-4.5 parts by weight.
[0024] The lithium salt includes one of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, or any mixture thereof.
[0025] The solvent includes one of ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, diethyl carbonate, propylene carbonate, and ethyl propionate, or any mixture thereof.
[0026] The additive includes one of vinylene carbonate, vinyl sulfate, lithium difluorooxalatoborate, and lithium difluorophosphate, or any mixture thereof.
[0027] The present invention also includes a battery, comprising the electrolyte.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The fluorosulfonyl carboxylate of the present invention can improve the film formation impedance of the battery, and the dense protective film of lithium fluoride formed by the fluorinated atoms can reduce the side reactions inside the battery; the thio group can further form an organic protective film on the outer layer of lithium fluoride, inhibit the oxidation reaction of the solvent under high voltage, and improve the overall high voltage resistance and cycle performance of the battery. At the same time, by regulating the length of the carboxylate segment or the number of carboxylate groups in the molecular structure, the high temperature performance of the battery can be taken into account while improving the low temperature, avoiding the influence of the increased viscosity on the battery performance. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.
[0031] A fluorosulfonyl carboxylate having a structure of formula (I);
[0032]
[0033] Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4.
[0034] Preferably, the R1 is selected from a molecular chain segment with 1-3 carbon atoms, and the value of n is 1-3; preferably, the R1 is methyl, ethyl, or isopropyl.
[0035] Preferably, the fluorosulfonyl carboxylate may be one of formulas (A1), (A2), (A3), and (A4).
[0036]
[0037]
[0038] The present invention also includes a method for preparing the fluorosulfonyl carboxylate, as shown in formula (II):
[0039]
[0040] Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4.
[0041] Specifically, the method comprises the following steps: under cooling conditions, gradually adding tetrafluoroethane-β-sultone to the R1-nOH alcohol substance; after the addition is completed, gradually returning the temperature to room temperature for reaction, and obtaining the product after treatment.
[0042] The molar ratio of tetrafluoroethane-β-sultone to the alcoholic hydroxyl group in the R1-nOH alcohol substance is 1:(1-1.2), specifically 1:1 or 1:1.2.
[0043] The specific treatment process is to blow away the residual hydrofluoric acid with nitrogen, wash the reaction mixture with water and brine, and collect the organic phase; then dry, filter and distill to obtain the final product.
[0044] The present invention also includes an electrolyte, comprising the fluorosulfonyl carboxylate, a solvent, a lithium salt and an additive. Preferably, the solvent accounts for 80-95 parts by weight, the lithium salt accounts for 12-15 parts by weight, the fluorosulfonyl carboxylate accounts for 0.5-6 parts by weight, and the additive accounts for 1.5-4.5 parts by weight.
[0045] Preferably, the solvent accounts for 85 parts by weight, the lithium salt accounts for 12 parts by weight, the fluorosulfonyl carboxylate accounts for 0.5-3 parts by weight, and the additive accounts for 2.5 parts by weight.
[0046] Preferably, the fluorosulfonyl carboxylate accounts for 0.5 parts by weight.
[0047] The lithium salt includes one of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, or any mixture thereof.
[0048] The solvent includes one of ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, diethyl carbonate, propylene carbonate, and ethyl propionate, or any mixture thereof.
[0049] The additive includes one of vinylene carbonate, vinyl sulfate, lithium difluorooxalatoborate, and lithium difluorophosphate, or any mixture thereof.
[0050] The present invention also includes a battery, comprising the electrolyte.
[0051] The following examples are used for illustration. Unless otherwise specified, the following weight parts are all in g.
[0052] Example 1
[0053] An electrolyte comprising the following components:
[0054] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 35 parts by weight of diethyl carbonate;
[0055] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0056] Fluorosulfonyl carboxylate: 0.5 parts by weight of A1;
[0057] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0058] Example 2
[0059] An electrolyte comprising the following components:
[0060] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 35 parts by weight of diethyl carbonate;
[0061] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0062] Fluorosulfonyl carboxylate: 0.5 parts by weight of A2;
[0063] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0064] Example 3
[0065] An electrolyte comprising the following components:
[0066] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 35 parts by weight of diethyl carbonate;
[0067] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0068] Fluorosulfonyl carboxylate: 0.5 parts by weight of A3;
[0069] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0070] Example 4
[0071] An electrolyte comprising the following components:
[0072] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 35 parts by weight of diethyl carbonate;
[0073] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0074] Fluorosulfonyl carboxylate: 0.5 parts by weight of A4;
[0075] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0076] Example 5
[0077] An electrolyte comprising the following components:
[0078] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 32 parts by weight of diethyl carbonate;
[0079] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0080] Fluorosulfonyl carboxylate: 3 parts by weight of A2;
[0081] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0082] Example 6
[0083] An electrolyte comprising the following components:
[0084] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 30 parts by weight of diethyl carbonate;
[0085] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0086] Fluorosulfonyl carboxylate: 6 parts by weight of A2;
[0087] Additives: 0.1 parts by weight of vinylene carbonate, 0.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0088] Comparative Example 1
[0089] An electrolyte comprising the following components:
[0090] Solvent: 25 parts by weight of ethylene carbonate, 25 parts by weight of ethyl methyl carbonate, 35 parts by weight of diethyl carbonate;
[0091] Lithium salt: 12 parts by weight of lithium hexafluorophosphate;
[0092] Additives: 0.1 parts by weight of vinylene carbonate, 1.3 parts by weight of vinyl sulfate, 0.6 parts by weight of lithium difluorooxalatoborate, and 0.5 parts by weight of lithium difluorophosphate.
[0093] Based on the electrolytes of Examples 1 to 6 and Comparative Example 1, a high voltage and low temperature resistant battery was further prepared. The specific preparation methods were as follows (except for the different formulations of the electrolytes, the others were the same):
[0094] Preparation of positive electrode sheet: Lithium iron phosphate, conductive agent CNT, carbon black and binder PVDF are evenly dispersed in NMP solvent at a mass ratio of 95.5:0.5:1.5:2.5. After stirring for a period of time under vacuum, the solid content of the positive electrode slurry is controlled at 62%. The positive electrode slurry is evenly coated on both surfaces of the aluminum foil, the electrode is dried, and the solid content is controlled at 3.2g / cm 3 It is compacted and rolled, and finally die-cut into specified sizes.
[0095] Preparation of negative electrode sheet: Graphite, carbon black, binder CMC and binder SBR are uniformly dispersed in deionized water at a mass ratio of 96.0:1.0:1.2:1.8. After being fully stirred in a vacuum, a uniformly mixed negative electrode slurry is obtained. The solid content of the negative electrode slurry is controlled at 50%. The negative electrode slurry is evenly coated on both surfaces of the negative electrode current collector copper foil, the electrode sheet is dried, and the temperature is set at 1.55g / cm 3 Compact and roll. Finally, cut into specified size for later use.
[0096] A polyethylene separator is used to combine the positive electrode sheet, the negative electrode sheet and the separator into a battery. After being placed in an aluminum-plastic film and dried, a shot of electrolyte is injected. After exhausting with a 0.1C current, the battery is prepared after packaging.
[0097] The following is a performance test of the batteries prepared with the electrolytes of Examples 1 to 6 and Comparative Example 1.
[0098] High voltage cycle performance test: At 25°C, the batteries prepared in Examples 1 to 6 and Comparative Example 1 were charged at a constant current rate of 1C. When the battery voltage reached 4.4V, they were switched to constant voltage charging until the current dropped to 0.05C and then stopped charging. After 10 minutes of dormancy, the batteries were discharged at a constant current rate of 1C until the battery voltage dropped to 2.8V and then stopped discharging. The batteries were dormant for 10 minutes. The above charging and discharging steps were repeated, and the cycle capacity retention rate of the battery was recorded.
[0099] Low temperature cycle test: At 0°C, the batteries prepared in Examples 1 to 6 and Comparative Example 1 were charged with constant current at a rate of 0.2C. When the battery voltage reached 4.4V, they were switched to constant voltage charging until the current dropped to 0.05C and then stopped charging. After 10 minutes of dormancy, the batteries were discharged with a constant current at a rate of 0.2C until the battery voltage dropped to 2.0V and then stopped discharging. The batteries were dormant for 10 minutes. The above charging and discharging steps were repeated, and the cycle capacity retention rate of the battery was recorded.
[0100] 60℃ high temperature storage experiment: At 25℃, the batteries prepared in Examples 1 to 6 and Comparative Example 1 were charged with constant current at a rate of 1C. When the battery voltage reached 4.4V, they were switched to constant voltage charging until the current dropped to 0.05C and the charging was stopped. The fully charged batteries were then placed in an oven at 60℃. After storage for 1 month, they were discharged at a rate of 1C at 25℃ to obtain the residual capacity. After that, they were charged and discharged again at a rate of 1C to obtain the recovery capacity after high temperature storage.
[0101] The test results of the batteries prepared using the electrolytes of Examples 1 to 6 and Comparative Example 1 are shown in Table 1 below.
[0102] Table 1: Test results of the time required for battery infiltration in various embodiments and comparative examples
[0103] High-voltage cycle results (capacity retention after 500 cycles) Example 1 87.7 Example 2 91.2 Example 3 89.9 Example 4 90.4 Example 5 87.1 Example 6 86.8 Comparative Example 1 85.9
[0104] Table 2: Test results of low temperature performance of batteries in various embodiments and comparative examples
[0105] The number of cycles required for the low temperature cycle capacity to decrease to 80% Example 1 47 Example 2 87 Example 3 70 Example 4 71 Example 5 46 Example 6 42 Comparative Example 1 38
[0106] Table 3: Residual capacity and recovery capacity of the batteries of each embodiment and comparative example after storage at 60°C
[0107]
[0108]
[0109] From Example 1, it can be found that after using fluorosulfonyl carboxylate, the overall high-voltage cycle capacity retention rate and low-temperature cycle capacity retention rate of the battery are improved to a certain extent. In Example 2, after A2 is added, the overall performance of the battery is optimal. This may be because the chain segment of this type of fluorosulfonyl carboxylate is longer and the degree of substitution is low. While improving high-temperature performance, the viscosity increases less. Example 5 and Example 6 compare the effects of different contents of fluorosulfonyl carboxylate on battery performance. It is found that excessive addition degrades battery performance. This may be because too much additive forms a larger interface impedance, affecting the performance of electrical properties.
[0110] It can be seen from the comparison between the above examples and comparative examples that the addition of fluorosulfonyl carboxylate can improve the overall high pressure resistance performance, and at the same time, the low temperature performance itself will also be improved.
[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A fluorosulfonyl carboxylate, characterized in that: Having the structure of formula (I); Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4.
2. The fluorosulfonyl carboxylate according to claim 1, characterized in that The R1 is selected from a molecular chain segment with 1-3 carbon atoms, and the value of n is 1-3; preferably, n is 1; preferably, the R1 is methyl, ethyl, or isopropyl.
3. A method for preparing the fluorosulfonyl carboxylate according to claim 1 or 2, characterized in that: As shown in formula (II): Wherein, R1 is selected from a molecular chain segment having 1-6 carbon atoms, and the value of n is 1-4, preferably, n is 1.
4. The preparation method according to claim 3, characterized in that: The method comprises the following steps: under cooling conditions, gradually adding tetrafluoroethane-β-sultone to the R1-nOH alcohol substance; after the addition is completed, gradually restoring the temperature to room temperature for reaction, and obtaining a product after treatment.
5. The preparation method according to claim 4, characterized in that: The treatment process is to blow away the residual hydrofluoric acid with nitrogen, wash the reaction mixture with water and brine, and collect the organic phase; then dry, filter and distill to obtain the final product.
6. An electrolyte, characterized in that: Comprising the fluorosulfonyl carboxylate according to claim 1 or 2, a solvent, a lithium salt and an additive; preferably, the solvent accounts for 80-95 parts by weight, the lithium salt accounts for 12-15 parts by weight, the fluorosulfonyl carboxylate accounts for 0.5-6 parts by weight, and the additive accounts for 1.5-4.5 parts by weight; Preferably, the fluorosulfonyl carboxylate accounts for 0.5-3 parts by weight, preferably 0.5 parts by weight.
7. The electrolyte according to claim 6, characterized in that The lithium salt includes one of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, or any mixture thereof.
8. The electrolyte according to claim 6, characterized in that The solvent includes one of ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, diethyl carbonate, propylene carbonate, and ethyl propionate, or any mixture thereof.
9. The electrolyte according to claim 6, characterized in that The additive includes one of vinylene carbonate, vinyl sulfate, lithium difluorooxalatoborate, and lithium difluorophosphate, or any mixture thereof.
10. A battery, characterized in that: The electrolyte comprising the electrolyte according to any one of claims 6 to 9.
Citation Information
Patent Citations
Fumigation method for preventing and controlling culture products from insects and mildew
CN106973901A
Fumigation method used for preventing and curing grain pests and mildew
CN106973990A
Electrolyte solution for secondary batteries, secondary battery, battery pack, electric vehicle and electronic device
CN109891653A
Polymer electrolyte composition comprising a fluorine-containing additive, and its use
DE102018217758A1
Cited By
Fluoro-sulfinate compound, preparation method and non-aqueous electrolyte
CN121824367A