Porous aromatic skeleton high-load metal composite material as well as preparation method and application thereof
Through the preparation of porous aromatic skeleton high-load metal composite materials, the problems of low metal load and poor stability of single atomic catalysts are solved, and efficient photocatalytic hydrogenation reaction is achieved, which significantly improves the stability and hydrogen production efficiency of the catalyst.
Patent Information
- Application Number
- CN202410966817.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, single-atom catalysts supported by metal organic frameworks have problems such as low metal loading, poor agglomeration and poor stability, which affect their catalytic activity and thermal stability.
The preparation method of porous aromatic skeleton high-load metal composite materials is adopted to synthesize bisphosphonium-based structured moieties and gold bisphosphonium-based structured moieties, and the electronegative nature of the skeleton phosphorus center is used to stabilize metal atoms, and metal loading is achieved through photocatalytic hydrogenation reaction Quantity regulation and stability improvement.
The metal loading and catalytic effect of single-atom catalysts are significantly improved, the agglomeration of metal atoms is avoided, the stability and hydrogen production efficiency of the catalyst are improved, and the rapid hydrogen evolution rate and the generation of high-quality hydrogen are achieved.
Smart Images

Figure CN118908995A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysis, and in particular relates to a porous aromatic skeleton high-load metal composite material and a preparation method and application thereof. Background Art
[0002] Single-atom catalysts are a type of heterogeneous metal catalysts with maximum atomic utilization and unsaturated coordination environment. They have good catalytic activity and selectivity, and have shown excellent performance in many fields such as photocatalysis, thermal catalysis, electrocatalysis, and biomimetic enzyme catalysis. However, due to the high surface energy of single-atom catalysts, they are very prone to agglomeration and deactivation during preparation and catalysis, which puts higher requirements on the synthesis of single-atom catalysts. However, single-atom catalysts loaded with metal organic frameworks (MOFs) and covalent organic frameworks (COFs) prepared by existing technologies still have some problems such as low metal loading, agglomeration and poor stability. Among them, too low metal loading affects the overall catalytic activity and catalytic efficiency of single-atom catalysts, which limits the practical application of the above-mentioned catalysts to a certain extent, that is, it is difficult to achieve simultaneous improvement of metal loading, catalytic effect and thermal stability. Therefore, how to simultaneously improve the metal loading, catalytic effect and thermal stability of single-atom catalysts while ensuring the dispersion of metal single atoms is a technical problem that needs to be solved urgently. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a porous aromatic skeleton high-load metal composite material, and its preparation method comprises the following steps:
[0004] (1) Synthesis of the bisphosphorus-based building block Bppe-4Br: Under nitrogen protection, p-bromoiodobenzene is placed in anhydrous tetrahydrofuran at 0 to 4°C and stirred until uniformly mixed, then 2 to 4 M isopropylmagnesium chloride is added, and the temperature is then lowered to -78 to -70°C, 1,2-(bis(dichlorophosphino)ethane) is added, and the mixture is stirred for 15 to 90 min, then the mixture is heated to room temperature, and deionized water is added after stirring at room temperature for 12 to 48 h. The mixture is extracted with ether to obtain an organic phase, and anhydrous sodium sulfate is added to the organic phase for drying. The product is purified by column chromatography to obtain a bisphosphorus-based ligand (Bppe-4Br), wherein the molar ratio of p-bromoiodobenzene: isopropylmagnesium chloride: 1,2-(bis(dichlorophosphino)ethane) is 2:2:1 to 8:8:1, and the structure of Bppe-4Br is as follows:
[0005]
[0006] (2) Synthesis of gold-bisphosphorus-based building block Au-Bppe-4Br: After mixing tetrahydrothiophene gold chloride and Bppe-4Br obtained in step (1), add dichloromethane and mix well, stir at room temperature for 15 to 90 minutes, then add ether after evaporation, wash with ether, filter and vacuum dry to obtain gold-bisphosphorus-based building block (Au-Bppe-4Br), wherein the molar ratio of tetrahydrothiophene gold chloride to Bppe-4Br is 1:2 to 3:1;
[0007] (3) 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine are mixed, and N,N-dimethylformamide is added to dissolve, and the activated reaction system 1 is obtained after stirring at room temperature for 15 to 120 minutes; any combination of Bppe-4Br or Au-Bppe-4Br is added to anhydrous tetrahydrofuran to completely dissolve, and then the activated reaction system 1 is added, and concentrated hydrochloric acid is added to quench the reaction after reacting at room temperature, and then the porous aromatic skeleton high-load metal composite material is obtained after washing with deionized water and tetrahydrofuran, and the tetrahydrofuran solution is extracted with Soxhlet for 12 to 24 hours;
[0008] The molar ratio of 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine is 1:1:1 to 3:1:1;
[0009] The molar ratio of Bppe-4Br to 1,5-cyclooctadiene is 1:8 to 1:5;
[0010] The molar ratio of Bppe-4Br, Au-Bppe-4Br and 1,5-cyclooctadiene is 0.1:0.01:1 to 0.5:0.3:3;
[0011] The molar ratio of Au-Bppe-4Br to 1,5-cyclooctadiene is 1:8 to 1:5.
[0012] The present invention also provides an application of a porous aromatic skeleton high-load metal composite material in a photocatalytic hydrogenation reaction, wherein the porous aromatic skeleton high-load metal composite material is added to a mixed solution of acetonitrile: water: triethanolamine, and under argon protection, at room temperature, hydrogen is obtained after irradiation with a xenon lamp for 0.5 to 48 hours, wherein the power of the xenon lamp is 150 to 300 W, and the wavelength range is 300 to 1100 nm;
[0013] The mass ratio of the porous aromatic skeleton high-load metal composite material to the mixed solution is 1:1100 to 1:800;
[0014] The volume ratio of acetonitrile: water: triethanolamine is 1:1:1 to 4:1:1.
[0015] Compared with the prior art, the advantages of the present invention are:
[0016] The present invention achieves the following excellent effects through the interaction between raw materials, ratio, process and synergistic regulation of parameters:
[0017] The present invention adopts an in-situ synthesis strategy at the molecular level to design and synthesize a new functional porous aromatic framework (PAFs) material. First, the role of the coordination site in the rigid framework is utilized. The high-content metal is stabilized by the abundant coordination sites in the framework and the ratio of the building blocks before and after metallization is changed to achieve adjustable and controllable metal loading, avoiding the phenomenon of related raw materials occupying the coordination center during the polymerization process, and maximizing the role of PAFs in stabilizing metal atoms. At the same time, the agglomeration of metal atoms caused by the high-temperature pyrolysis deposition method is avoided. In the application of photocatalytic hydrogen evolution, a rapid hydrogen evolution rate and increased hydrogen evolution quality can be achieved at the same time. The specific analysis is as follows:
[0018] (1) Compared with existing single-atom catalysts, the metal loading of the single-atom catalyst prepared by the present invention is significantly increased, and there is no metal atom agglomeration phenomenon.
[0019] (2) The present invention uses PAFs materials as carriers for the first time to prepare high-load single-atom catalysts, designs and synthesizes new diphosphorus monomers and performs metallization, and uses the strong electronegativity of the skeleton phosphorus center to stabilize the metal atoms. The rigid skeleton structure of the PAFs material fully exposes the coordination sites, achieving the purpose of stabilizing high-density metal atoms. Similarly, the high stability and porosity of the PAFs material can reduce the metal leaching rate of the single-atom catalyst and promote the transport of substances in the catalytic process.
[0020] (3) The preparation method provided by the present invention has controllable metal loading of the single-atom catalyst, and the metal loading is controlled by utilizing the synergistic control effect of the interaction, ratio, process and parameters between the raw materials.
[0021] (4) The high-load single-atom catalyst prepared by the present invention is applied to photocatalytic hydrogen production, which can simultaneously achieve rapidity and increase the quality of hydrogen evolution. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 a and 1b are respectively the steps (1) and (2) of Example 1 of the present invention to obtain the diphosphorus-based ligand Bppe-4Br and the gold diphosphorus-based building block Au-Bppe-4Br. 1 H NMR spectrum;
[0023] Figure 2 a and 2b are respectively the steps (1) and (2) of Example 1 of the present invention to obtain the diphosphorus-based ligand Bppe-4Br and the gold diphosphorus-based building block Au-Bppe-4Br. 31 P NMR spectrum;
[0024] Figure 3 a and Figure 3 c are Au provided in Examples 3 and 5 of the present invention respectively 5% -SAs-PAF-164 and Au 100% - Spherical aberration electron microscope comparison of SAs-PAF-164, Figure 3 b and 3d are Au provided in Examples 3 and 5 of the present invention. 5% -SAs-PAF-164 and Au 100% - Comparison of element distribution of SAs-PAF-164;
[0025] Figure 4 a and Figure 4 b are Au provided in Examples 3 and 5 of the present invention respectively. 5% -SAs-PAF-164 and Au 100% -SAs-PAF-164 synchrotron radiation X-ray absorption spectrum comparison chart, among which, Figure 4 a and Figure 4 b The horizontal axis represents Space bond length, ordinate represents the Fourier transform of k-space;
[0026] Figure 5 The Au obtained in Examples 3, 4 and 5 of the present invention 5% -SAs-PAF-164, Au 50% -SAs-PAF-164 and Au 100% -Comparison chart of photocatalytic hydrogen evolution effect of SAs-PAF-164. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not limit the present invention.
[0028] Embodiment 1:
[0029] In this embodiment, the specific steps for preparing the diphosphorus-based ligand Bppe-4Br and the gold diphosphorus-based building block Au-Bppe-4Br are as follows:
[0030] (1) Synthesis of Bppe-4Br: Under nitrogen protection, p-bromoiodobenzene was placed in anhydrous tetrahydrofuran at 0°C and stirred until uniformly mixed, and then 2M isopropylmagnesium chloride was added. The system temperature was lowered to -78°C, 1,2-(bis(dichlorophosphino)ethane) was added, stirred for 30 minutes, then the temperature was raised to room temperature, and stirred at room temperature for 12 hours. After completion, deionized water was added to the system, and ether was used for extraction to obtain an organic phase, and anhydrous sodium sulfate was added to the organic phase for drying. The product was purified by column chromatography to obtain a bisphosphino ligand (Bppe-4Br), and the molar ratio of p-bromoiodobenzene: isopropylmagnesium chloride: 1,2-(bis(dichlorophosphino)ethane) was 4:4:1.
[0031] (2) Synthesis of Au-Bppe-4Br: After mixing tetrahydrothiophene gold chloride and Bppe-4Br obtained in step (1), add dichloromethane and mix well, stir at room temperature for 30 minutes, then add ether after evaporation, wash with ether, filter and vacuum dry to obtain gold diphosphine building block (Au-Bppe-4Br). The molar ratio of tetrahydrothiophene gold chloride to Bppe-4Br is 2:1.
[0032] like Figure 1 a and Figure 1 b, respectively, Bppe-4Br and Au-Bppe-4Br 1 H NMR spectrum; Figure 2 a and Figure 2 b are Bppe-4Br and Au-Bppe-4Br respectively. 31 P NMR spectrum. The above results prove that the gold diphosphorus-based building block was successfully synthesized, that is, the diphosphorus-based ligand was successfully metallized.
[0033] Embodiment 2:
[0034] 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine were mixed in a molar ratio of 1.5:1.46:1.46, and N,N-dimethylformamide was added to dissolve, and the mixture was stirred at room temperature for 30 minutes to obtain an activation reaction system 1. Bppe-4Br obtained in step (1) of Example 1 was added to anhydrous tetrahydrofuran to completely dissolve, and then the mixture was mixed with the activation reaction system 1 and reacted at room temperature for 48 hours, and then concentrated hydrochloric acid was added to quench the reaction, and then washed with deionized water and tetrahydrofuran, and extracted with tetrahydrofuran solution for 24 hours to obtain a PAFs material (PAF-164). The molar ratio of Bppe-4Br to 1,5-cyclooctadiene was 0.28:1.5.
[0035] Embodiment 3:
[0036] 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine were mixed in a molar ratio of 1.5:1.46:1.46, and N,N-dimethylformamide was added to dissolve them. After stirring at room temperature for 30 minutes, an activation reaction system 1 was obtained. Bppe-4Br obtained in step (1) of Example 1 and Au-Bppe-4Br obtained in step (2) were added to anhydrous tetrahydrofuran to completely dissolve, and then mixed with the activation reaction system 1 and reacted at room temperature for 48 hours. After that, concentrated hydrochloric acid was added to quench the reaction, and then washed with deionized water and tetrahydrofuran, and extracted with tetrahydrofuran solution for 24 hours to obtain a porous aromatic skeleton high-load metal composite material 1 (Au 5% -SAs-PAF-164 catalyst), the actual metal loading was measured to be 3.5wt% by inductively coupled plasma characterization. The molar ratio of Bppe-4Br, Au-Bppe-4Br and 1,5-cyclooctadiene was 0.266:0.014:1.5.
[0037] Embodiment 4:
[0038] 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine were mixed in a molar ratio of 1.5:1.46:1.46, and N,N-dimethylformamide was added to dissolve them. After stirring at room temperature for 30 minutes, an activation reaction system 1 was obtained. Bppe-4Br obtained in step (1) of Example 1 and Au-Bppe-4Br obtained in step (2) were added to anhydrous tetrahydrofuran to completely dissolve them. Then, they were mixed with the activation reaction system 1 and reacted at room temperature for 48 hours. After that, concentrated hydrochloric acid was added to quench the reaction. After washing with deionized water and tetrahydrofuran, and Soxhlet extraction with the tetrahydrofuran solution for 24 hours, a porous aromatic skeleton high-load metal composite material 2 (Au 50% -SAs-PAF-164 catalyst), the metal loading was measured to be 30.8wt% by inductively coupled plasma characterization. The molar ratio of Bppe-4Br, Au-Bppe-4Br and 1,5-cyclooctadiene was 0.14:0.14:1.5.
[0039] Embodiment 5:
[0040] 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine were mixed in a molar ratio of 1.5:1.46:1.46, and N,N-dimethylformamide was added to dissolve, and the activated reaction system 1 was obtained after stirring at room temperature for 30 minutes. The Au-Bppe-4Br obtained in step (2) of Example 1 was added to anhydrous tetrahydrofuran to completely dissolve, and then it was mixed with the activated reaction system 1 and reacted at room temperature for 48 hours, and then concentrated hydrochloric acid was added to quench the reaction, and then washed with deionized water and tetrahydrofuran, and the tetrahydrofuran solution was extracted with Soxhlet for 24 hours to obtain a porous aromatic skeleton high-load metal composite material 3 (Au 100% -SAs-PAF-164 catalyst), the metal loading was measured to be 45.3wt% by inductively coupled plasma characterization. The molar ratio of Au-Bppe-4Br to 1,5-cyclooctadiene was 0.28:1.5.
[0041] like Figure 3 a and Figure 3 c, Au prepared from Examples 3 and 5 5% -SAs-PAF-164 and Au 100% - In the spherical aberration electron microscope image of SAs-PAF-164, bright spots can be clearly observed, which are Au atoms loaded in PAF-164. Figure 3 There are many bright spots in c, indicating that the Au 100% -SAs-PAF-164 has a high metal loading density and no agglomeration occurs. Figure 3 Spherical aberration electron microscopy shows that porous aromatic framework high-loaded metal composite materials have been successfully synthesized. Figure 3 b and Figure 3 d Proof Au 5% -SAs-PAF-164 and Au 100% -SAs-PAF-164 elements are evenly distributed on the material skeleton. Figure 4 a and Figure 4 b shows the coordination structure of Au single atoms in the porous aromatic skeleton high-load metal composite material, where the Au 5% -SAs-PAF-164 is composed of two P atoms in the framework jointly anchoring Au atoms, while the Au prepared in Example 5 100% -SAs-PAF-164 has a high metal loading, and each P atom in the framework anchors one Au atom.
[0042] Embodiment 6:
[0043] In this example, PAF-164 prepared in Example 2 is added to a mixed solution of acetonitrile: water: triethanolamine, wherein the volume ratio of acetonitrile: water: triethanolamine is 3:1:1, and hydrogen is obtained after irradiation with a xenon lamp for 1-5 hours at room temperature under argon protection. The mass ratio of PAF-164 to the mixed solution is 1:900; the power of the xenon lamp is 300W, and the wavelength range is 400-1100nm.
[0044] Embodiment 7:
[0045] In this example, the Au prepared in Example 3 5% -SAs-PAF-164 catalyst is added to a mixed solution of acetonitrile: water: triethanolamine, wherein the volume ratio of acetonitrile: water: triethanolamine is 3:1:1, and under argon protection, at room temperature, it is illuminated by xenon light for 1-5 hours to obtain hydrogen. 5% -The mass ratio of SAs-PAF-164 to the mixed solution is 1:900; the power of the xenon lamp is 300W, and the wavelength range is 400-1100nm.
[0046] Embodiment 8:
[0047] In this example, the Au prepared in Example 4 50% -SAs-PAF-164 catalyst is added to a mixed solution of acetonitrile: water: triethanolamine, wherein the volume ratio of acetonitrile: water: triethanolamine is 3:1:1, and under argon protection, at room temperature, it is illuminated by xenon light for 1-5 hours to obtain hydrogen. 50% -The mass ratio of SAs-PAF-164 to the mixed solution is 1:900; the power of the xenon lamp is 300W, and the wavelength range is 400-1100nm.
[0048] Embodiment 9:
[0049] In this example, the Au prepared in Example 5 100% -SAs-PAF-164 catalyst is added to a mixed solution of acetonitrile: water: triethanolamine, wherein the volume ratio of acetonitrile: water: triethanolamine is 3:1:1, and under argon protection, at room temperature, it is illuminated by xenon light for 1-5 hours to obtain hydrogen. 100% -The mass ratio of SAs-PAF-164 to the mixed solution is 1:900; the power of the xenon lamp is 300W, and the wavelength range is 400-1100nm.
[0050] Compared with the amount of hydrogen released in Example 6, the amount of hydrogen released in Examples 7-9 is larger, which proves that the porous aromatic skeleton high-load metal composite material obtained in the present invention has excellent photocatalytic hydrogen release performance. Figure 5As shown, with the increase of illumination time, the Au 5% -SAs-PAF-164, Au 50% -SAs-PAF-164 and Au 100% -SAs-PAF-164 gradually increases the amount of hydrogen released, and with the increase of Au content in the catalyst, the mass of hydrogen released increases significantly. 100% -SAs-PAF-164 was used as the catalyst, and the amount of hydrogen released after 1-5 hours of illumination was 4.82-15.86 mmol / g. 5% -SAs-PAF-164 and Au 50% -SAs-PAF-164 photocatalysts have hydrogen evolution amounts of 0.59-6.96 and 2.41-10.36 mmol / g, respectively.
[0051] Comparative Example 1:
[0052] Jiang Hailong's research group published a research paper titled "Platinum Atom Catalyst Confined in Metal-Organic Framework for High-Efficiency Photocatalysis". The prior art is to confine a single Pt atom in MOF by using the pore size of MOF, and to obtain a single-atom catalyst Al-TCPP-Pt by using the confinement effect of MOF, wherein the content of loaded Pt single atom is 0.29wt%. It can be seen that the porous aromatic skeleton high-loaded metal composite material 1 (Au 5% -SAs-PAF-164 catalyst) has a minimum metal loading (3.5 wt%) much higher than Al-TCPP-Pt (0.29 wt%). Similarly, under the same catalytic conditions as in Example 1, after 4 h of catalytic reaction, the amount of hydrogen released by Al-TCPP-Pt is 0.724 mmol g -1 , which is lower than the hydrogen evolution amount of the single-atom Au catalyst supported on PAFs prepared in Examples 3-5 of the present invention in 3 h (the hydrogen evolution amounts of the catalysts in Examples 3-5 in 3 h catalysis (time shorter than the time disclosed in Comparative Example 1) are 2.59, 8.18 and 13.75 mmol g -1 ), and at the same time, it is also lower than the amount of hydrogen evolution with the same or other longer illumination time as the present invention. (Adv.Mater.2018,30,1705112)
[0053] Comparative Example 2:
[0054] The research group of Zhang Jinlong and Xi Xinguo reported a research paper titled "Platinum single atoms anchored on a covalent organic framework: active sites that promote photocatalytic hydrogen evolution". The prior art is to anchor single Pt atoms on the pore walls of a covalent organic framework (TpPa-1-COF) connected to two-dimensional β-ketoamines, and the single atom catalyst Pt1@TpPa-1 prepared in this way has a metal loading of 0.72wt%. The single Pt atoms in Pt1@TpPa-1 serve as catalytic active sites, wherein the metal loading is lower than that of the single atom catalysts obtained in Examples 3-5 of the present invention, and the hydrogen evolution of the single atom catalysts obtained in the present invention within only 5 hours of reaction (respectively 6.96, 10.36 and 15.86 mmol / g) are all higher than the hydrogen evolution of Pt1@TpPa-1 disclosed in Comparative Example 2 when the reaction is 6 hours (5.5 mmol g -1 ). (ACS Catal.2021,11,13266-13279)
[0055] Table 1 Comparison of metal loading and hydrogen evolution of the single atom catalysts prepared in Examples 3-5 and the catalysts in the comparative examples
[0056]
[0057]
[0058] In summary, the present invention and the comparative example use different framework materials, and when Au and Pt are respectively used for compounding with different framework materials, the minimum loading amount of the Au catalyst obtained by the present invention is much higher than the Pt catalyst disclosed in the prior art. In the process of photocatalytic hydrogenation, the present invention uses a shorter time than the prior art, and the amount of hydrogen precipitation obtained is much higher than the amount of hydrogen precipitation obtained by the prior art. Compared with the prior art, the present invention breaks the bottleneck that the single-atom catalyst of the prior art is very easy to agglomerate and deactivate, and realizes the use of the strong interaction between the carrier and the metal atom to achieve the purpose of stabilizing the metal atom. The catalyst finally obtained has good catalytic efficiency, high stability, and significantly shortens the catalytic hydrogen production reaction time. Under the same catalytic hydrogen production reaction conditions, a catalytic speed higher than that disclosed in the prior art is achieved, that is, a large amount of reaction time is saved, and the prepared hydrogen content is much higher than the hydrogen content obtained by the prior art, thereby improving the hydrogen production efficiency. In addition, the three different catalysts obtained in Examples 3-5 of the present invention show different effects in the catalytic hydrogen production reaction, from which it is concluded that the catalyst performance and application of different structures obtained by the present invention are also different. In summary, the present invention achieves the best effects of catalyst stability, high hydrogen production efficiency and other performances through the coordinated regulation of components, ratios, processes and process parameters. The present invention adopts a molecular level pre-coordination strategy to construct a PAFs-loaded single-atom catalyst. Through the coordinated regulation of the above-mentioned raw material interactions, ratios, processes and process parameters, and only within the scope of protection of the claims of the present invention, can the ratio of metallized building units be effectively regulated, and finally the metal catalytic sites and metal loading in the catalyst be effectively controlled, and stability is improved. Breakthrough the limitations of the mutual restriction of the loading of single-atom catalysts and the dispersion behavior of metal atoms, that is, breaking the technical bottleneck of the prior art metal atom loading, metal atom dispersion, and stability that are difficult to maintain effective regulation, effectively controlling the migration of metal atoms and inhibiting agglomeration, promoting the transmission and separation of substances in the catalytic process, and improving the catalytic efficiency of single-atom catalysts, and simultaneously improving the loading and stability of single-atom catalysts, achieving effective dispersion of metal atoms, shortening the catalytic time, and increasing the amount of hydrogen produced. Compared with the prior art, the present invention simultaneously improves the metal loading, catalytic effect, and thermal stability of single-atom catalysts, and thus achieves significant technical effects.
[0059] The embodiments described above are detailed descriptions of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and do not limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A porous aromatic skeleton high-load metal composite material, the preparation method of which comprises the following steps: (1) Synthesis of the bisphosphorus-based building block Bppe-4Br: Under nitrogen protection, p-bromoiodobenzene is placed in anhydrous tetrahydrofuran at 0 to 4°C and stirred until uniformly mixed, then 2 to 4 M isopropylmagnesium chloride is added, and the temperature is then lowered to -78 to -70°C, 1,2-(bis(dichlorophosphino)ethane) is added, and the mixture is stirred for 15 to 90 min, then the mixture is heated to room temperature, and deionized water is added after stirring at room temperature for 12 to 48 h. The mixture is extracted with ether to obtain an organic phase, and anhydrous sodium sulfate is added to the organic phase for drying. The product is purified by column chromatography to obtain a bisphosphorus-based ligand (Bppe-4Br), wherein the molar ratio of p-bromoiodobenzene: isopropylmagnesium chloride: 1,2-(bis(dichlorophosphino)ethane) is 2:2:1 to 8:8:1, and the structure of Bppe-4Br is as follows: (2) Synthesis of gold-bisphosphorus-based building block Au-Bppe-4Br: After mixing tetrahydrothiophene gold chloride and Bppe-4Br obtained in step (1), add dichloromethane and mix well, stir at room temperature for 15 to 90 minutes, then add ether after evaporation, wash with ether, filter and vacuum dry to obtain gold-bisphosphorus-based building block (Au-Bppe-4Br), wherein the molar ratio of tetrahydrothiophene gold chloride to Bppe-4Br is 1:2 to 3:1; (3) After mixing 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine, N,N-dimethylformamide was added to dissolve, and the activated reaction system 1 was obtained after stirring at room temperature for 15 to 120 minutes; any combination of Bppe-4Br or Au-Bppe-4Br was added to anhydrous tetrahydrofuran to completely dissolve, and then the activated reaction system 1 was added. After reacting at room temperature, concentrated hydrochloric acid was added to quench the reaction, and then the porous aromatic skeleton high-load metal composite material was obtained after washing with deionized water and tetrahydrofuran and Soxhlet extraction with tetrahydrofuran solution for 12 to 24 hours.
2. The porous aromatic skeleton high-load metal composite material according to claim 1, characterized in that: The molar ratio of 1,5-cyclooctadiene, bis(1,5-cyclooctadiene)nickel(0) and 2,2'-bipyridine in step (3) is 1:1:1 to 3:1:
1.
3. The porous aromatic skeleton high-load metal composite material according to claim 1, characterized in that: The molar ratio of Bppe-4Br to 1,5-cyclooctadiene in step (3) is 1:8 to 1:
5.
4. The porous aromatic skeleton high-load metal composite material according to claim 1, characterized in that: The molar ratio of Bppe-4Br, Au-Bppe-4Br and 1,5-cyclooctadiene in step (3) is 0.1:0.01:1 to 0.5:0.3:
3.
5. The porous aromatic skeleton high-load metal composite material according to claim 1, characterized in that: The molar ratio of Au-Bppe-4Br to 1,5-cyclooctadiene in step (3) is 1:8 to 1:
5.
6. Application of the porous aromatic skeleton high-load metal composite material according to claims 1-5 in photocatalytic hydrogenation reaction, characterized in that: The preparation method comprises: adding a porous aromatic skeleton high-load metal composite material into a mixed solution of acetonitrile: water: triethanolamine, and irradiating with a xenon lamp for 0.5 to 48 hours at room temperature under argon protection to obtain hydrogen, wherein the power of the xenon lamp is 150 to 300 W and the wavelength range is 300 to 1100 nm; The mass ratio of the porous aromatic skeleton high-load metal composite material to the mixed solution is 1:1100 to 1:800; The volume ratio of acetonitrile: water: triethanolamine is 1:1:1 to 4:1:1.