Tetrazine energetic material as well as preparation method and application thereof
By designing and synthesizing MC2HxN10Oy crystals with ClO4-ion-free tetrazine energy-containing material MC2HxN10Oy crystals, the problems of environmental pollution and high laser ignition thresholds in laser detonation ignition technology are solved, and the laser detonation effect with low laser initiation thresholds and high performance is achieved. Important commercial application value.
Patent Information
- Application Number
- CN202410916820.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-09
AI Technical Summary
In the existing laser detonation ignition technology, energy-containing materials containing ClO4-ions have great harm to environmental pollution and human health, and the laser ignition threshold is high, making it difficult to meet the needs of safe and efficient detonation.
Design and synthesize a tetrazine-energic material MC2HxN10Oy crystal. By selecting metal salt and 3,6-dihydrazine-1,2,4,5-tetrazine as ligand, reacting with nitric acid solvent, it is prepared without containing Laser-responsive sensitive material of ClO4-ion, with low laser initiation threshold and low environmental pollution.
The laser detonation materials with low laser initiation threshold, low environmental pollution and high performance have been achieved, and the problems of ClO4-ion pollution and high laser ignition threshold have been overcome, and they have important commercial application value.
Smart Images

Figure CN118909001A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a tetrazine energetic material and a preparation method and application thereof, belonging to the technical field of laser detonation and ignition. Background Art
[0002] Laser ignition technology has become a new type of ignition technology developed in recent years and has received more and more attention. As a new type of ignition technology, laser ignition technology has the advantages of high output energy, high ignition efficiency, high controllability, and high safety. By combining laser ignition technology with energetic materials, the safety and reliability of the use of ignition technology in the current complex external environment can be greatly improved. Therefore, it is very important to study the application of laser ignition technology in the field of energetic materials. Energetic coordination compounds (ECCs) have rich assembly modes and more flexible designs, so they have become a research hotspot for scientific researchers in the field of laser ignition. A large number of ECCs that can be used for laser ignition have been reported. However, these ECCs usually contain ClO4 - Ions, such as [(TriTzPyr)3Fe][ClO4]2, [Fe(MTZ)6](ClO4)2, Cu(H2DAPZCA)2(ClO4)4·2H2O, Cu(HAPZCA)2(ClO4)4, etc. ClO4 - Ion pollution of water environment has become one of the most serious environmental problems. - Ions are also harmful to human health, especially thyroid function, which in turn affects human metabolism. Based on the above reasons, the goal of this application is to design and synthesize a class of laser-responsive and ClO4-free - ions, a new type of ECCs that is environmentally friendly. Summary of the invention
[0003] According to one aspect of the present application, a tetrazine energetic material is provided as a laser detonation ignition charge, the laser detonation ignition energy required is generally lower than that of the reported compounds, and the serious ClO4 - Despite the disadvantages of ion contamination and high laser ignition threshold, it has important commercial application value in the field of laser detonation and ignition.
[0004] The tetrazine energetic material described in the present application includes MC2H x N 10 O y Crystals;
[0005] M is selected from any one of Mn, Fe, Co, Cu, Zn, Cd and Ni;
[0006] When M is selected from any one of Mn, Fe, Co, Cu, Zn and Cd, x=8, y=7;
[0007] When M is Ni, x=10, y=8.
[0008] Optionally, the MC2H x N 10 O y The structure of the crystal is a 0D fullerene-like planar structure.
[0009] Optionally, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The crystals belong to the P1 space group;
[0010] When M is Ni, the MC2H x N 10 O y The crystals belong to the P21 / c space group.
[0011] Optionally, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74~78°; β=81~85°; γ=80~84°; Z=0.4~0.6.
[0012] Preferably, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74.5~77.0°; β=81.5~84.9°; γ=80.5~83.5°; Z=0.5.
[0013] Preferably, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74.80~77.25°; β=81.8~84.90°; γ=80.70~83.50°;
[0014]
[0015] Optionally, when M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are:
[0016] α=85~93°; β=90~93°; γ=87~93°;
[0017] Z=0.4~0.6.
[0018] Preferably, when M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are:
[0019] α=87.5~92.5°; β=90.5~93.0°;
[0020] γ=88.5~92.50°; Z=0.5.
[0021] Preferably, when M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are:
[0022] α=88.20~91.50°;
[0023] β=91.50~93.0°; γ=89.00~91.50°;
[0024] Optionally, the MC2H x N 10 O y The nitrogen content of the crystal is 33-43%; the decomposition temperature is 100-105°C; the impact sensitivity is 3-5J; the friction sensitivity is 60-175N; and the electrostatic spark sensitivity is 40-45mJ.
[0025] In another aspect, the present application provides a method for preparing the energetic material, comprising: reacting a mixture including a metal salt containing M, a ligand, and a solvent to obtain the energetic material;
[0026] The M is selected from any one of Mn, Fe, Co, Cu, Zn, Cd and Ni;
[0027] The ligand is 3,6-dihydrazino-1,2,4,5-tetrazine.
[0028] Optionally, the M-containing metal salt is selected from any one or more of M-containing perchlorates, nitrates, and halogen-containing metal salts.
[0029] Optionally, the solvent is nitric acid.
[0030] Optionally, the molar ratio of the metal salt containing M to the ligand is (1-3): (1-4);
[0031] The molar number of the metal salt containing M is calculated based on the molar number of M.
[0032] Optionally, the concentration of the nitric acid is 10-35wt%; preferably, the concentration of the nitric acid is 15-30wt%.
[0033] Optionally, the added amount of the M-containing metal salt and the solvent is (20-120) mg: (5-20) mL.
[0034] Optionally, the added amounts of the M-containing metal salt and the solvent are independently selected from any value of 75 mg: 8 mL, 80 mg: 15 mL, 30 mg: 10 mL, 60 mg: 10 mL, 25 mg: 5 mL, 120 mg: 8 mL, 60 mg: 20 mL, 20 mg: 5 mL, 20 mg: 20 mL, 120 mg: 5 mL, 120 mg: 20 mL, or a range between any two of the above.
[0035] Optionally, the reaction temperature is 25-60°C.
[0036] Optionally, the reaction temperature is independently selected from any one of 25°C, 35°C, 45°C, 50°C, 60°C or a range between any two of the above.
[0037] In another aspect, the present application provides a use of the energetic material as a laser detonation ignition charge.
[0038] The beneficial effects of this application include:
[0039] 1) The energetic material provided in this application has a simple synthesis method, a very low laser initiation threshold, and is environmentally friendly. Experimental determination shows that the impact sensitivity of the compound is no higher than 5J, the friction sensitivity is no higher than 175N, and the electrostatic spark sensitivity is within the range of 40-45mJ.
[0040] 2) The energetic material described in this application is lower than most of the currently reported laser detonation ignition materials and does not contain ClO4 – Ions have important commercial application value in the field of green high-performance energetic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 For this application CuC2H8N10 Powder diffraction pattern of O7;
[0042] Figure 2 For this application CuC2H8N 10 Crystal structure diagram of O7;
[0043] Figure 3 For this application NiC2H 10 N 10 Crystal structure diagram of O8;
[0044] Figure 4 CuC2H8N 10 O7 hot pin test picture;
[0045] Figure 5 This is a schematic diagram of the laser detonation ignition test device;
[0046] Figure 6 CuC2H8N 10 Schematic diagram of O7 used as laser detonation ignition charge when the laser energy is 4.2mJ. DETAILED DESCRIPTION
[0047] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0048] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0049] N a The calculation method of % is:
[0050] T dec b , IS c , FS d 、ESD e The testing instruments are TGA / DSC 1 / 1100 thermogravimetric analyzer, BFH-12 impact sensitivity meter, FSKM-10 friction sensitivity meter and Xspark 8 electrostatic spark sensitivity tester.
[0051] The powder diffraction instrument was a Rigaku Miniflex 600 powder X-ray diffractometer.
[0052] The hot needle test method is to place a 20 mg sample in a loose state on a copper plate and trigger it with a high-temperature iron needle heated under a Bunsen burner for 3 minutes.
[0053] Example 1
[0054] Compound MnC2H8N 10The synthesis method of O7 is as follows: Mn(NO3)2·4H2O (75.30 mg) and ligand DHT (14.21 mg) were added to 8 mL of 30% mass fraction nitric acid solvent, and the mixture was reacted at 45°C for 72 hours, and then cooled to room temperature and filtered to obtain a large amount of MnC2H8N 10 O7 dark brown crystals.
[0055] The MnC2H8N 10 The structure of O7 dark brown crystal is a 0D fullerene-like planar structure.
[0056] Example 2
[0057] Compound FeC2H8N 10 The synthesis method of O7 is as follows: Fe(NO3)3·9H2O (80.80 mg) and ligand DHT (42.63 mg) were added to 16 mL of 20% mass fraction nitric acid solvent, and the mixture was reacted at 35°C for 96 hours, and then cooled to room temperature and filtered to obtain a large amount of FeC2H8N 10 O7 black crystal.
[0058] The FeC2H8N 10 The structure of O7 black crystal is a 0D fullerene-like planar structure.
[0059] Example 3
[0060] Compound CoC2H8N 10 The synthesis method of O7 is as follows: Co(NO3)2·6H2O (29.10 mg) and ligand DHT (28.42 mg) were added to 10 mL of 15% mass fraction nitric acid solvent, and the mixture was reacted at 45°C for 96 hours, and then cooled to room temperature and filtered to obtain a large amount of chemical formula CoC2H8N 10 O7 deep red crystals.
[0061] The CoC2H8N 10 The structure of O7 deep red crystal is a 0D fullerene-like planar structure.
[0062] Example 4
[0063] Compound NiC2H 10 N 10 The synthesis method of O8 is as follows: Ni(NO3)2·6H2O (58.16 mg) and ligand DHT (14.21 mg) were added into 10 mL of 15% mass fraction nitric acid solvent, and the mixture was reacted at 25°C for 24 hours, and then cooled to room temperature and filtered to obtain a large amount of NiC2H 10 N 10O8 reddish brown crystals.
[0064] Figure 3 NiC2H 10 N 10 The crystal structure diagram of O8, which has a 0D fullerene-like planar structure.
[0065] Example 5
[0066] Compound CuC2H8N 10 The synthesis method of O7 is as follows: Cu(NO3)2·3H2O (24.16 mg) and ligand DHT (14.21 mg) were added to 5 mL of 15% mass fraction nitric acid solvent, and the mixture was reacted at 25°C for 24 hours, and then cooled to room temperature and filtered to obtain a large amount of CuC2H8N 10 O7 black crystal.
[0067] Figure 1 CuC2H8N 10 The powder diffraction pattern of O7 shows that the spectrum measured by the experimental instrument is highly consistent with the spectrum obtained by crystal data simulation, indicating that the compound samples used in the experiment are all pure samples, ensuring the reliability of the samples used in subsequent tests.
[0068] Figure 2 CuC2H8N 10 The crystal structure diagram of O7, which has a 0D fullerene-like planar structure.
[0069] Figure 4 20mgCuC2H8N 10 O7 hot needle test diagram. From the figure, it can be seen that the high-temperature hot needle heated by the Bunsen burner is 10 Upon contact, O7 immediately began to produce smoke, followed by a bright flame of a gigantic size.
[0070] Figure 5 Figure 1 is a schematic diagram of the laser detonation ignition test device. To determine the minimum laser initiation threshold E (E = P × T) of the sample, the sample (about 20 mg) was placed in an Al2O3 crucible and the pulse power (P = 3 W) and pulse intensity (I = 15.3 W cm) were determined within a certain T (pulse duration) range. -2 ) to irradiate it. As T decreases, the output laser energy (E) also decreases accordingly. After multiple experiments, the critical energy at which the sample can be accurately triggered, that is, the minimum laser triggering threshold, is finally determined.
[0071] Figure 6 20mg CuC2H8N recorded 10O7 is used as the laser ignition charge when the laser energy is 4.2mJ. As can be seen from the figure, CuC2H8N 10 O7 was successfully ignited and detonated, with a large, bright flame clearly observed.
[0072] Example 6
[0073] Compound ZnC2H8N 10 The synthesis method of O7 is as follows: Zn(NO3)2·6H2O (119.00 mg) and ligand DHT (14.21 mg) were added to 8 mL of 25% mass fraction nitric acid solvent, and the mixture was reacted at 50°C for 120 hours, and then cooled to room temperature and filtered to obtain a large amount of ZnC2H8N 10 O7 deep red crystal.
[0074] The ZnC2H8N 10 The structure of O7 deep red crystal is a 0D fullerene-like planar structure.
[0075] Example 7
[0076] Compound CdC2H8N 10 The synthesis method of O7 is as follows: Cd(NO3)2·4H2O (61.70 mg) and ligand DHT (14.21 mg) were added to 20 mL of 25% mass fraction nitric acid solvent, and the mixture was reacted at 60°C for 36 hours, and then cooled to room temperature and filtered to obtain a large amount of CdC2H8N 10 O7 black crystal.
[0077] The CdC2H8N 10 The structure of O7 black crystal is a 0D fullerene-like planar structure.
[0078] The relevant crystallographic parameters of the above crystals are shown in Table 1.
[0079] Table 1
[0080]
[0081] Table 1
[0082]
[0083] The performance parameters of the above crystals are shown in Table 2.
[0084] Table 2
[0085]
[0086] Among them, N a = nitrogen content; T decb = decomposition temperature; IS c = Impact sensitivity; FS d = Friction sensitivity; ESD e = Static spark sensitivity.
[0087] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A tetrazine energetic material, characterized in that: Including MC2H x N 10 O y Crystals; M is selected from any one of Mn, Fe, Co, Cu, Zn, Cd and Ni; When M is selected from any one of Mn, Fe, Co, Cu, Zn and Cd, x=8, y=7; When M is Ni, x=10, y=8.
2. The tetrazine energetic material according to claim 1, characterized in that: The MC2H x N 10 O y The structure of the crystal is a 0D fullerene-like planar structure.
3. The tetrazine energetic material according to claim 1, characterized in that: When M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The crystals belong to the P1 space group; When M is Ni, the MC2H x N 10 O y The crystals belong to the P21 / c space group.
4. The tetrazine energetic material according to claim 1, characterized in that: When M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74~78°; β=81~85°; γ=80~84°; Z = 0.4-0.6; Preferably, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74.5~77.0°; β=81.5~84.9°; γ=80.5~83.5°; Z = 0.5; Preferably, when M is selected from any one of Mn, Fe, Co, Cu, Zn, and Cd, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=74.80~77.25°; β=81.8~84.90°; γ=80.70~83.50°; 5. The tetrazine energetic material according to claim 1, characterized in that: When M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=85~93°; β=90~93°; γ=87~93°; Z = 0.4-0.6; Preferably, when M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=87.5~92.5°; β=90.5~93.0°; γ=88.5~92.50°; Z = 0.5; Preferably, when M is Ni, the MC2H x N 10 O y The unit cell parameters of the crystal are: α=88.20~91.50°; β=91.50~93.0°; γ=89.00~91.50°; 6. The tetrazine energetic material according to claim 1, characterized in that: The MC2H x N 10 O y The nitrogen content of the crystal is 33-43%; the decomposition temperature is 100-105°C; the impact sensitivity is 3-5J; the friction sensitivity is 60-175N; and the electrostatic spark sensitivity is 40-45mJ.
7. A method for preparing the tetrazine energetic material according to any one of claims 1 to 6, characterized in that: include: reacting a mixture including a metal salt containing M, a ligand, and a solvent to obtain the energetic material; The M is selected from any one of Mn, Fe, Co, Cu, Zn, Cd and Ni; The ligand is 3,6-dihydrazino-1,2,4,5-tetrazine.
8. The method for preparing the tetrazine energetic material according to claim 7, characterized in that: The metal salt containing M is selected from any one or more of perchlorates, nitrates, and halogen-containing metal salts containing M; Preferably, the solvent is nitric acid.
9. The method for preparing the tetrazine energetic material according to claim 7, characterized in that: The molar ratio of the metal salt containing M to the ligand is (1-3): (1-4); The molar number of the metal salt containing M is calculated based on the molar number of M; Preferably, the concentration of the nitric acid is 10-35wt%; Preferably, the added amount of the metal salt containing M and the solvent is (20-120) mg: (5-20) mL; Preferably, the reaction temperature is 25-60°C.
10. Use of the tetrazine energetic material according to any one of claims 1 to 6 as laser detonation ignition powder, propellant or additive.
Citation Information
Patent Citations
BTATz Energetic Metal Complexes and Their Preparation Methods
CN102267982A
Di-hydrazino-s-tetrazine decahydro decaborate compound
CN102827093A
Energetic compounds and compositions
CN107074819A
1,5-dinitramino tetrazolyl dihydrazino tetrazine salt compound
CN107698532A
Low-nitrogen energetic complex as well as preparation method and application thereof
CN114478591A
Cited By
Gem-dinitrotetrazole energetic material as well as preparation method and application thereof
CN121159466A