Method for preparing super absorbent resin by adopting reversed-phase suspension polymerization

Through the reverse phase suspension polymerization method and the design of surfactant, the problems of limited surface area of ​​highly absorbent resin particles and poor granulation performance of fine powder are solved, efficient water absorption performance and particle size distribution optimization are achieved, and the process flow is simplified.

CN118909198AInactive Publication Date: 2024-11-08JIANGSU SAILBOAT PETROCHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410997873.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing preparation process of highly absorbent resins has limited geometric shapes of spherical particles, resulting in the inability to increase the surface area, bottlenecks in pure water absorption performance, large performance losses in fine powder granulation process, poor water retention performance, and uneven drying, which affects product performance.

Method used

Using reverse phase suspension polymerization method, different surfactants are prepared by controlling the HLB value to prepare different surfactants, forming a uniform suspension system, performing multiple polymerizations and surface crosslinking, realizing deep crosslinking and agglomeration molding , reduce moisture content and improve particle strength and particle size distribution.

Benefits of technology

A higher water absorption ratio is achieved, the cross-linking strength and particle size distribution of particles are improved, the powder generation rate is reduced, the conversion rate and water absorption performance of the product are improved, and the process flow is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909198A_ABST
    Figure CN118909198A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing super absorbent resin by adopting reversed-phase suspension polymerization. The method comprises the following steps: step 1, preparing a nonionic surfactant; 2, preparing a polymerization solution; step 3, polymerizing; step 4, carrying out surface crosslinking; two composite nonionic surfactants are adopted, ethylene oxide is controlled to be added for multiple times during preparation of nonionic block polyether, two polymerization products with high and low primary hydroxyl content are prepared, and two polymerization products with different HLB values are further obtained. The surfactant b1 has the characteristic of low HLB (Hydrophile-Lipophile Balance) value, and can uniformly disperse the polymerization liquid into single micro-spheres. The surfactant b2 has a high HLB value and can obviously reduce the surface tension between particles, meanwhile, under the action of osmotic pressure difference, the surface layer of the first-section polymer particles can absorb part of the second-section polymer liquid to achieve osmotic pressure balance, in the second-section polymerization reaction process, deep cross-linking and interpenetrating can be achieved between first-section polymer gel ion molecular chains and second-section polymer gel ion molecular chains, and the surface tension between the first-section polymer gel ion molecular chains and the second-section polymer gel ion molecular chains can be reduced. And the cross-linking strength among the agglomerated basic particles is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin preparation, in particular to a method for preparing a highly water-absorbent resin by adopting reverse phase suspension polymerization. Background Art

[0002] The polymerization process of super absorbent resin is mainly divided into aqueous solution polymerization and suspension polymerization. The aqueous solution polymerization method is further divided into kettle process, kneader process and belt process, etc. The super absorbent resin prepared by each process has its own characteristics.

[0003] Super absorbent polymer (SAP) is a moderately cross-linked polymer compound with a three-dimensional network structure that can absorb hundreds or even thousands of times its own amount of water. Due to its strong ability to absorb water and retain moisture under pressure, it is widely used in diapers, sanitary napkins, pet pads, water-blocking materials for cables, and water-retaining agents for agriculture and forestry.

[0004] Chinese invention CN201410010153.4 is a water-absorbent resin suitable for sanitary materials. It adopts a two-step or multi-step intermittent reverse suspension polymerization process, adds an aqueous unsaturated monomer solution to petroleum hydrocarbons to construct a reverse suspension system, cools down after the first-step reverse polymerization to allow the dispersant to precipitate, then adds a two-step unsaturated monomer aqueous solution for agglomeration and two-step suspension polymerization, then dehydrates and removes petroleum hydrocarbons, and finally dries to obtain the desired highly absorbent resin. The water-absorbent resin particles obtained by this reverse suspension production process are spherical agglomerates. Due to the limitation of the geometric shape of the sphere, the specific surface area cannot be further improved, and there is a bottleneck in the pure water absorption performance.

[0005] China Invention CN201980032452.9 water-absorbent resin powder and its manufacturing method, through two processes of drying and fine powder granulation, the drying process dries the water-containing gel into particles, the key of the present invention is mainly in the fine powder granulation process, the fine powder produced by grinding in the production line is mixed with the granulation aid (including cross-linking agent) by the fine powder granulation equipment to obtain granules, and then the fine powder granules are mixed with the normal granulation granules to achieve the purpose of recovering the fine powder. The fine powder recovery process has many disadvantages: the performance of the fine powder is greatly lost after granulation, and the water retention and absorption performance are very poor, which affects the product performance; after the fine powder is granulated, it will enter the grinding system to produce fine powder again, resulting in a large amount of fine powder in the system circulation; after the fine powder is granulated, the granules are smaller than the normal granulation granules, which is easy to cause uneven drying or over-drying. For this reason, a method for preparing highly absorbent resin by reverse suspension polymerization is provided. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a highly absorbent resin by inverse suspension polymerization in view of the defects of the prior art, so as to solve the problems raised by the above-mentioned background technology.

[0007] To achieve the above object, the present invention provides the following technical solution: a method for preparing a highly absorbent resin by inverse suspension polymerization, the specific steps of which are as follows:

[0008] Step 1: Preparation of nonionic surfactant;

[0009] 2-ethyl-1-heptanol is used as an initiator, 48%-50% potassium hydroxide is used as a catalyst, the amount of the catalyst is 0.5%-2% of the amount of the initiator, negative pressure dehydration is performed at 100° C.-150° C., after a certain amount of water is removed, ethylene oxide of the total mass of the reaction is added to perform a first addition reaction, propylene oxide is added after the reaction is completed, and finally ethylene oxide is added to obtain a block polyether, and surfactants with different HLB values ​​are prepared according to different addition numbers of ethylene oxide;

[0010] Among them, the HLB value of 1-11 is used for the suspension system gel protective agent b1, and the HLB value of 15-20 is used for the hydrophilic surfactant b2 for agglomerating the gel particles;

[0011] Step 2: Preparation of polymerization solution;

[0012] Step 2.1: Preparation of a polymerization solution;

[0013] Acrylic acid, sodium hydroxide and desalted water are mixed and stirred to prepare an unsaturated monomer aqueous solution, and an initiator and a cross-linking agent are added and stirred evenly to obtain a first-stage polymerization solution;

[0014] Step 2.2: Preparation of the second stage polymerization solution;

[0015] Acrylic acid, sodium hydroxide, desalted water, and a hydrophilic surfactant b2 for agglomerating gel particles are mixed and stirred to prepare a water-soluble unsaturated monomer aqueous solution, and the mixture is stirred evenly to obtain a second-stage polymerization solution;

[0016] Step 3: Aggregation;

[0017] After the reactor is evacuated, add the suspension system gel protective agent b1 and the organic dispersing solvent in sequence; after fully dissolving for 10-60 minutes, add a polymerization liquid, stir at a high speed of 200-300r / min to form a uniform suspension system, maintain the mixing time for 10-60 minutes, set the oil bath temperature to 80-90℃ to initiate the polymerization reaction; when the mixed solution in the reactor changes from milky white to transparent, cool the polymerization oil bath and set the oil bath temperature to 20-30℃; after the system in the reactor reaches 20-30℃, add The second stage polymerization liquid treated by pre-cooling is stirred stably for 10-60 minutes, and the stirring speed is 300-400r / min; after reaching the set stirring time, the high temperature oil bath is turned on again to initiate the secondary polymerization, and the oil bath temperature is set to 80-90°C to initiate the polymerization reaction. After the reaction is completed, negative pressure distillation is performed. After the solid content reaches 85-95%, the oil bath is cooled by 40-50°C, and the materials in the kettle are placed in a flat plate centrifuge for solid-liquid separation, and finally uniform basic particles are obtained, and the average particle size distribution is concentrated in 40-55 meshes;

[0018] Step 4: surface cross-linking;

[0019] The separated basic particles are placed in a vacuum drying oven for vacuum devolatilization for 20-60 minutes, with a vacuum degree of 30-60 kPa; after treatment, the particles are placed in a coating machine for surface coating operation, and then heated to 140-150°C to complete the surface cross-linking reaction, and the moisture of the particles is further dried to finally obtain finished particles.

[0020] As a preferred technical solution of the present invention, the initiator in step 2.1 is a persulfate inorganic thermal initiator and one or more of 2,2'-azobis(2-imidylpropane) dihydrochloride, 2,2'-azobis(2-methylpropionamide) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[2-(2-imidazoline-2-yl)propane] dihydrochloride, and 2,2'-azobis(2-methylpropylimidamide) dihydrochloride, and the total amount added is 0.02%-0.30% of the mass of the acrylic acid monomer in the neutralization solution.

[0021] As a preferred technical solution of the present invention, the cross-linking agent in step 2.1 is one or two of polyethylene glycol diacrylate, pentaerythritol triacrylate, pentaerythritol triallyl ether, dipentaerythritol pentaacrylate, ethoxylated trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated neopentyl glycol diacrylate, triethoxylated glycerol triacrylate, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, trimethylolethane triglycidyl ether, 1,4-butanediol diglycidyl ether, and N,N-methylenebisacrylamide, and the added mass is 0.02%-0.50% of the mass of the acrylic acid monomer in the neutralizing solution.

[0022] As a preferred technical solution of the present invention, the mass concentration of acrylic acid in the first stage polymerization solution and the second stage polymerization solution in step 2 is 25%-45%, and the neutralization molar ratio is 60%-85%.

[0023] As a preferred technical solution of the present invention, the mass ratio of the second-stage polymerization liquid to the first-stage polymerization liquid in the polymerization liquid used in step 3 is 0.4-1.

[0024] As a preferred technical solution of the present invention, the mass ratio of the second-stage polymerization liquid to the first-stage polymerization liquid is 0.55-0.6.

[0025] As a preferred technical solution of the present invention, the amount of the suspension system gel protective agent b1 added in step 3 is 0.01%-2.00% of the mass of the organic dispersing solvent; the organic dispersing solvent is one or a mixture of straight-chain alkanes and cycloalkanes.

[0026] As a preferred technical solution of the present invention, the straight-chain alkane is n-hexane or n-heptane; the cycloalkane is cyclohexane or cyclopentane.

[0027] As a preferred technical solution of the present invention, in step 3, the second-stage polymerization liquid needs to be pre-cooled before being added to the reactor, and the temperature control range is 10°C-40°C.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. Two composite nonionic surfactants are used. By controlling the addition of ethylene oxide in multiple times during the preparation of nonionic block polyether, two high and low primary hydroxyl contents are prepared, and then two polymerization products with different HLB values ​​are obtained. Surfactant b1 has the characteristics of low HLB value and good dispersibility, and can evenly disperse the polymerization liquid into a single microsphere. Surfactant b2 has a higher HLB value, which can significantly reduce the surface tension between particles. At the same time, under the action of osmotic pressure difference, the surface layer of the first-stage polymerization particles will absorb part of the second-stage polymerization liquid to achieve osmotic pressure balance. In this way, during the second-stage polymerization reaction, the first-stage and second-stage polymerization gel ion molecular chains can achieve deep crosslinking and interpenetration, so that the crosslinking strength between the agglomerated basic particles is higher, and a better agglomeration molding effect is achieved. The agglomerated particles can still maintain their original shape without breaking even under a certain pressure state.

[0030] 2. The particle size distribution can be freely changed by changing the feed temperature of the second-stage polymerization liquid, the conversion rate of the first-stage polymer, the speed of the first-stage agitator, and the speed of the second-stage agitator to meet the needs of different particle size distributions.

[0031] 3. The water absorption rate of the super absorbent resin sample prepared by this method is 1.5-2 times that of the conventional absorbent resin in 1 minute. At the same time, it has great advantages over conventional SAP in centrifugal water retention, residual monomers and absorption speed.

[0032] 4. The water content and residual acrylic acid monomers are reduced by azeotropic devolatilization under reduced pressure. After the reaction, the basic material is loose agglomerated solid particles, which makes it easier to separate the particles from the dispersion medium. At the same time, the sample has extremely low residual acrylic acid monomers. This effectively avoids the adhesion between particles of the basic hydrogel particles due to the stickiness of the gel surface in the polymerization-first-separation-and-drying method, which is not conducive to subsequent drying, particle dispersion, and removal of residual dispersion medium.

[0033] 5. The surface cross-linking process is carried out outside the reactor, which can realize the continuous operation of the surface cross-linking process. During the heating cross-linking reaction, the moisture content of the finished particles is further reduced, which effectively improves the utilization rate of the polymerization reactor and the energy utilization efficiency of the surface cross-linking process, and the process flow is more concise and efficient;

[0034] 6. The higher the powder content of the super absorbent resin particles with a particle size of less than 150 μm, the easier it is to generate dust during use, which affects the use environment and also causes a certain degree of material loss. In the agglomerated resin particles prepared by this method, the first and second stage polymerized particles achieve deeper and more efficient cross-linking and interpenetration, effectively improving the particle agglomeration rate, and the yield of particles > 150 μm in the finished particles can reach more than 95%, thereby significantly reducing the generation rate of powder particles < 150 μm and improving the conversion rate of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 : Appearance image of the sample of Example 1 of the present invention magnified 800 times. DETAILED DESCRIPTION

[0036] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0037] Preparation of hydrophobic surfactant b1:

[0038] Use 300g 2-ethyl-1-heptanol as the initiator and 2.7g 49% potassium hydroxide as the catalyst in a 3L polymerization reactor, perform negative pressure dehydration at 100°C for 1h, add 338g ethylene oxide at 135°C to perform the first addition reaction, and slowly add 449g propylene oxide after the reaction is complete. Degas the intermediate by heating, and add 30g ethylene oxide at 145°C to obtain a block polyether surfactant b1 with an HLB value of 9 after the reaction.

[0039] Preparation of hydrophilic surfactant b2:

[0040] Use 300g 2-ethyl-1-heptanol as the initiator and 2.7g 49% potassium hydroxide as the catalyst in a 3L polymerization reactor, carry out negative pressure dehydration at 100°C for 1h, add 698g ethylene oxide at 135°C to carry out the first addition reaction, and after the reaction is complete, slowly add 41g propylene oxide, degas the intermediate by heating, add 81g ethylene oxide at 145°C, and after the reaction, obtain a block polyether surfactant b2 with an HLB value of 19.

[0041] Example 1: After 703.4g of acrylic acid was diluted with 1456.0g of desalted water, 544.2g of 50% sodium hydroxide was added dropwise in an ice-water bath while stirring for neutralization reaction. After the reaction was complete, 5.7g of sodium persulfate and 3.74g of pentaerythritol triacrylate were added and stirred to obtain 2703.5g of a first-stage polymerization liquid. After 406.2g of acrylic acid was diluted with 610.4g of desalted water, 336.7g of 50% sodium hydroxide was added dropwise in an ice-water bath while stirring for neutralization reaction. After the reaction was complete, 3.1g of sodium persulfate, 1.6g of polyethylene glycol 600 diacrylate and 0.49g of surfactant b2 were added and stirred to obtain 1355.6g of a second-stage polymerization liquid.

[0042] In a 20L stirred reactor equipped with a reflux condenser, the pressure was reduced to negative pressure, 4500g of cyclohexane was sucked in, 18.5g of surfactant b was added, the oil bath was raised to 50°C for thorough mixing for 10min, 2703.5g of the first stage polymerization liquid was added, the stirring speed was 180r / min, a suspension polymerization system was formed, and after mixing for 30min, the water bath was raised to 85°C for polymerization reaction. Azeotropic steam was formed in the gas phase space in the reactor, and condensed water was separated after reflux condensation. After the first stage polymerization temperature reached 74°C, the high-temperature oil bath was stopped for 10min and the normal temperature circulating oil bath was switched to 30°C. When the temperature in the 20L polymerization reactor reached 35°C, the low-temperature circulation was stopped. 1355.6g of the second-stage polymerization liquid was treated with nitrogen and then added to a 20L reactor. The stirring speed was adjusted to 260r / min. After stabilization for 10 minutes, the 85°C oil bath was turned on again to initiate secondary polymerization. The oil bath lasted for 3.5 hours, and 2293.5g of water was separated, accounting for 91.7% of the total water volume of the system. Then the water bath was stopped, and the materials in the reactor were separated into solid and liquid. After vacuum devolatilization of the separated basic particles, 1503.4g of basic agglomerated particles were obtained, with a water content of 8.2%. Finally, the obtained basic agglomerated particles were sprayed with surface coating liquid in a coating machine for surface coating operation, and the surface cross-linking reaction was completed after heating in an oven for 10 minutes, and finally 1428.4g of agglomerated finished particles were obtained. The apparent state of the product was agglomerated grape spheres.

[0043] Example 2: Based on Example 1, when the temperature in the 20L polymerization reactor reaches 30°C, the low temperature circulation is stopped. The second stage stirring speed is adjusted from 260r / min to 450r / min, and the operation of Example 1 is repeated. The appearance of the product is agglomerated grape spheres.

[0044] Example 3: Based on Example 1, when the polymer in the first stage reactor reaches 40°C, the low temperature cycle is stopped. The second stage polymerization liquid is added to the reactor, and the operation of Example 1 is repeated. The appearance of the product is agglomerated grape spheres.

[0045] Example 4: Based on Example 1, the surfactant b2 in the second-stage polymerization solution was adjusted from 0.49 g to 0.351 g, and the operation of Example 1 was repeated. The appearance of the product was agglomerated grape spheres.

[0046] Example 5: Based on Example 1, when the conversion rate of the first-stage polymer reaches 98%, the high-temperature oil bath is stopped and the low-temperature circulating oil bath is switched to 40°C. When the polymer in the first-stage reactor reaches 45°C, the low-temperature circulation is stopped. The second-stage polymerization liquid is added to the reactor, and the operation of Example 1 is repeated. The appearance of the product is agglomerated grape spheres.

[0047] Example 6: Based on Example 1, the self-made gel protective agent b1 was replaced with sucrose fatty acid ester S-1170, the high temperature oil bath was stopped and the low temperature circulating oil bath was switched to 40°C, and when the polymer in the first stage kettle reached 45°C, the low temperature circulation was stopped. The operation of Example 1 was repeated, and the appearance of the product was agglomerated grape spheres.

[0048] Example 7: Based on Example 1, the crosslinking agent pentaerythritol triacrylate in the first stage of the polymerization solution was replaced by ethylene glycol diglycidyl ether, and the homemade gel protective agent b1 was replaced by Span 20. When the polymer temperature in the first stage of the reactor was adjusted from 35°C to 45°C, the low-temperature cycle was stopped. The operation of Example 1 was repeated later, and the appearance of the product was agglomerated grape spheres. The disadvantage was that the material had a Span odor that was not easy to remove.

[0049] Comparative Example 1: Based on Example 1, the surfactant b2 in the second-stage polymerization solution was removed. The operation of Example 1 was repeated, and the appearance of the product was micro-powder.

[0050] Comparative Example 2: Based on Example 1, after the polymerization temperature reaches 74°C, the high temperature oil bath is stopped for 10 minutes and the low temperature circulating oil bath is switched to 10°C. When the temperature in the 20L polymerization kettle reaches 15°C, the low temperature circulation is stopped.

[0051] The deoxygenated second stage polymerization liquid was added, and the operation of Example 1 was repeated, and the first stage polymer was agglomerated and demulsified after stirring for 5 minutes.

[0052] Comparative Example 3: Based on Example 1, the surfactant b2 in the second-stage polymerization liquid was adjusted from 0.49 g to 1.485 g, and the operation of Example 1 was repeated. After stirring for a certain period of time, the first-stage polymer agglomerates and demulsifies.

[0053] Comparative Example 4: Based on Example 1, when the conversion rate of the first-stage polymer reaches 95%, the high-temperature oil bath is stopped and the low-temperature circulating oil bath is switched to 30°C. When the polymer in the first-stage reactor reaches 35°C, the low-temperature circulation is stopped. The second-stage polymerization liquid is added to the reactor, and the operation of Example 1 is repeated. After stirring for a certain period of time, the first-stage polymer is agglomerated and demulsified.

[0054] Comparative Example 5: Based on Example 1, 406.2 g of acrylic acid was diluted with 610.4 g of desalted water, and then 336.7 g of 50% sodium hydroxide was added dropwise in an ice-water bath while stirring for neutralization reaction. After the reaction was complete, 3.1 g of sodium persulfate and 1.6 g of polyethylene glycol 600 diacrylate were added, and then stirred evenly to obtain 1355.6 g of a first-stage polymerization liquid. 703.4 g of acrylic acid was diluted with 1456.0 g of desalted water, and then 544.2 g of 50% sodium hydroxide was added dropwise in an ice-water bath while stirring for neutralization reaction. After the reaction was complete, 5.7 g of sodium persulfate and 3.74 g of polyethylene glycol 600 diacrylate were added, and then stirred evenly to obtain 2703.5 g of a second-stage polymerization liquid. The operation of Example 1 was repeated later, and the appearance of the product was micro-powder.

[0055] It can be seen from the embodiments, comparative examples and Table 1 that:

[0056] After the polymerization, surfactant b1 is added to the system, which contains a small amount of hydroxyl non-ionic block polymer, and its HLB value is preferably controlled to be 3-11. Surfactant b2 is added to the system, which contains a large amount of hydroxyl non-ionic block polymer, and its HLB value is preferably controlled to be 15-20. This reduces the surface tension of a section of polymer particles and plays a role in "demulsification", causing its protective isolation function to be partially lost, and the particles adhere to each other to form organic / inorganic hybrid agglomerated particles. The average particle size can be adjusted according to the mass fraction of the added inorganic particles to meet the requirements of SAP particle size in different fields.

[0057] Table 1: Analytical data of Examples 1-7 compared with Comparative Examples 1-4

[0058]

[0059]

[0060] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention.

Claims

1. A method for preparing a super absorbent resin by reverse phase suspension polymerization, characterized in that: The specific steps are as follows: Step 1: Preparation of nonionic surfactant; 2-ethyl-1-heptanol is used as an initiator, 48%-50% potassium hydroxide is used as a catalyst, the amount of the catalyst is 0.5%-2% of the amount of the initiator, negative pressure dehydration is performed at 100° C.-150° C., after a certain amount of water is removed, ethylene oxide of the total mass of the reaction is added to perform a first addition reaction, propylene oxide is added after the reaction is completed, and finally ethylene oxide is added to obtain a block polyether, and surfactants with different HLB values ​​are prepared according to different addition numbers of ethylene oxide; Among them, the HLB value of 1-11 is used for the suspension system gel protective agent b1, and the HLB value of 15-20 is used for the hydrophilic surfactant b2 for agglomerating the gel particles; Step 2: Preparation of polymerization solution; Step 2.1: Preparation of a polymerization solution; Acrylic acid, sodium hydroxide and desalted water are stirred and mixed to prepare an unsaturated monomer aqueous solution, and an initiator and a cross-linking agent are added and stirred evenly to obtain a first-stage polymerization liquid; Step 2.2: Preparation of the second stage polymerization solution; Acrylic acid, sodium hydroxide, desalted water, and a hydrophilic surfactant b2 for agglomerating gel particles are stirred and mixed to prepare a water-soluble unsaturated monomer aqueous solution, and stirred evenly to obtain a second-stage polymerization solution; Step 3: Aggregation; After the reactor is evacuated, add the suspension system gel protective agent b1 and the organic dispersing solvent in sequence; after fully dissolving for 10-60 minutes, add a polymerization liquid, stir at a high speed of 200-300r / min to form a uniform suspension system, maintain the mixing time for 10-60 minutes, set the oil bath temperature to 80-90℃ to initiate the polymerization reaction; when the mixed solution in the reactor changes from milky white to transparent, cool the polymerization oil bath and set the oil bath temperature to 20-30℃; after the system in the reactor reaches 20-30℃, add The second stage polymerization liquid treated by pre-cooling is stirred stably for 10-60 minutes, and the stirring speed is 300-400r / min; after reaching the set stirring time, the high temperature oil bath is turned on again to initiate the secondary polymerization, and the oil bath temperature is set to 80-90°C to initiate the polymerization reaction. After the reaction is completed, negative pressure distillation is performed. After the solid content reaches 85-95%, the oil bath is cooled by 40-50°C, and the materials in the kettle are placed in a flat plate centrifuge for solid-liquid separation, and finally uniform basic particles are obtained, and the average particle size distribution is concentrated in 40-55 meshes; Step 4: surface cross-linking; The separated basic particles are placed in a vacuum drying oven for vacuum devolatilization for 20-60 minutes, with a vacuum degree of 30-60 kPa; after treatment, the particles are placed in a coating machine for surface coating operation, and then heated to 140-150°C to complete the surface cross-linking reaction, and the moisture of the particles is further dried to finally obtain finished particles.

2. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: The initiator described in step 2.1 is a persulfate inorganic thermal initiator and one or more of 2,2'-azobis(2-imidylpropane) dihydrochloride, 2,2'-azobis(2-methylpropionamide) dihydrochloride, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[2-(2-imidazoline-2-yl)propane] dihydrochloride, and 2,2'-azobis(2-methylpropylimidamide) dihydrochloride, and the total amount added is 0.02%-0.30% of the mass of the acrylic acid monomer in the neutralization solution.

3. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: The cross-linking agent in step 2.1 is one or two of polyethylene glycol diacrylate, pentaerythritol triacrylate, pentaerythritol triallyl ether, dipentaerythritol pentaacrylate, ethoxylated trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated neopentyl glycol diacrylate, triethoxylated glycerol triacrylate, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, trimethylolethane triglycidyl ether, 1,4-butanediol diglycidyl ether, and N,N-methylenebisacrylamide, and the added mass is 0.02%-0.50% of the mass of the acrylic acid monomer in the neutralization solution.

4. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: In step 2, the mass concentration of acrylic acid in the first stage polymerization liquid and the second stage polymerization liquid is 25%-45%, and the neutralization molar ratio is 60%-85%.

5. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: In the polymerization liquid used in step 3, the mass ratio of the second-stage polymerization liquid to the first-stage polymerization liquid is 0.4-1.

6. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 5, characterized in that: The mass ratio of the second stage polymerization liquid to the first stage polymerization liquid is 0.55-0.

6.

7. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: In step 3, the amount of the suspension system gel protective agent b1 added is 0.01%-2.00% of the mass of the organic dispersing solvent; the organic dispersing solvent is one or a mixture of straight-chain alkanes and cycloalkanes.

8. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 7, characterized in that: The straight-chain alkane is n-hexane or n-heptane; the cycloalkane is cyclohexane or cyclopentane.

9. The method for preparing a super absorbent resin by inverse suspension polymerization according to claim 1, characterized in that: In step 3, the second stage polymerization liquid needs to be pre-cooled before being added to the reactor, and the temperature control range is 10°C-40°C.

Citation Information

Patent Citations

  • Super absorbent polymer (SAP) prepared by one-step reversed phase suspension polymerization and preparation method of SAP

    CN107522991A

  • Reversed phase suspension polymerization preparation technology of water absorbent resin

    CN109535307A

  • Method of preparing water-absorbing resin

    CN1146997A

  • Super absorbent resin and preparation method thereof

    CN116178614A

  • Method for producing highly absorbing resin

    JP2005126474A