Preparation method of PVA optical film with excellent stretchability

By adding carbon dots to form a double cross-linked network during the preparation of PVA optical films, the problem of easy breakage during thinning was solved, the tensile properties were improved, and other excellent properties were maintained.

CN118909281APending Publication Date: 2024-11-08ANHUI WANWEI ADVANCED FUNCTIONAL MEMBRANE MATERIALS RESEARCH INSTITUTE CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411109282.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

PVA optical films are prone to breakage during the thinning process. The existing grain size is large and non-uniform, which leads to stress concentration during stretching, making it difficult to improve stretchability while ensuring other properties.

Method used

By adding carbon dots during the preparation of PVA optical films, a double cross-linked network is formed. The nano-effect of carbon dots is used to form micro-crosslinks with PVA molecular chains, thereby enhancing the toughness and tensile properties of the film.

Benefits of technology

It significantly improves the elongation at break of PVA optical films and enhances tensile properties, while having minimal impact on other properties, thus avoiding the performance losses caused by existing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991694070000081
    Figure BDA0004991694070000081
  • Figure BDA0004991694070000091
    Figure BDA0004991694070000091
Patent Text Reader

Abstract

The invention discloses a preparation method of a PVA optical film with excellent stretchability, and belongs to the technical field of PVA optical films. The preparation method of the PVA optical film comprises the following steps: (1) dissolving PVA resin and an additive in a solvent, and doping carbon dots to prepare a film casting stock solution; (2) uniformly mixing the casting membrane stock solution, extruding and defoaming, and carrying out tape casting through a die head to obtain a semi-finished product; and (3) pre-drying the semi-finished product by a drying guide roller, and drying and shaping the semi-finished product in a heat treatment oven to obtain the PVA optical film. The PVA optical film prepared by the invention has excellent tensile property on the premise of less influence on optical property by selecting a PVA value with proper polymerization degree and carbon dots with proper particle size to prepare a film casting stock solution, adjusting the proportion of the carbon dots in the film casting stock solution and utilizing the cross-linking toughening effect of the carbon dots and PVA resin, and solves the problem of film breakage in the stretching processing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVA optical films, and in particular relates to a method for preparing a PVA optical film with excellent stretchability. Background Art

[0002] Polyvinyl alcohol (PVA) is a water-soluble high molecular polymer made from vinyl acetate by polymerization and alcoholysis. It is not only simple to prepare and low-cost, but also has excellent hydrophilicity, gas barrier properties, acid and alkali resistance, organic solvent resistance, outstanding biosafety and good film-forming ability. Polyvinyl alcohol optical film is mainly used in the production of polarizers, and the end products are various types of liquid crystal displays, such as televisions, computer monitors, mobile phones, car navigation and display panels for wearable electronic devices. In recent years, with the continuous thinning of mobile phones, computers and liquid crystal displays, higher requirements have been put forward for the thinning of PVA films. However, thin PVA films are prone to breakage during the stretching process, which may be related to the large grain size and poor phase domain uniformity in the film. The structural non-uniformity can easily cause stress concentration during the stretching process, resulting in wrinkles or even breaks in the film during the iodine dyeing and stretching process.

[0003] The processing of PVA optical film adopts the cast film processing technology. After the PVA solution system is dissolved in the dissolving kettle, it is extruded through the extruder and the die, gradually dried on the casting roller and the drying roller, and finally formed into a product through heat treatment. The crystal morphology structure of the film, such as the crystal size and uniformity, determines the stretchability and film breaking of the film in the downstream stretching process. Therefore, how to reduce the crystal size and improve the uniformity of the crystal size is the key to solving the problems of easy film breaking in the downstream processing of thin PVA optical base film.

[0004] In the existing methods, the uniformity of the internal structure of the material can be improved by grain refinement, which has a certain effect on improving tensile properties. However, this method usually leads to the loss of other properties and the emergence of other problems, such as poor dyeing performance and more surface defects. Therefore, other ways are needed to improve the uniformity of the internal network structure of the material and improve the tensile properties. The adjustment of the formula usually does not have a big impact on the process and has little impact on other properties. It is a good choice to improve the tensile properties and ensure the excellent performance of other comprehensive properties. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a PVA optical film with excellent stretchability, so as to improve the stretchability of the PVA optical film.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a PVA optical film with excellent stretchability comprises the following steps:

[0008] (1) dissolving PVA resin and additives in a solvent and adding carbon dots to prepare a film casting solution;

[0009] (2) mixing the film casting stock solution uniformly, extruding and degassing it, and casting it through a die head to obtain a semi-finished product;

[0010] (3) The semi-finished product is pre-dried by a drying guide roller and then placed in a heat treatment oven for drying and shaping to obtain a PVA optical film.

[0011] Furthermore, the thickness of the PVA optical film is less than 45 μm.

[0012] Furthermore, the average particle size of the carbon dots is 5nm-50nm, preferably 10nm-25nm.

[0013] If the particle size of carbon dots is too small, the number of sites for interaction between carbon dots and PVA molecular chains will decrease, and the cross-linking effect will decrease, which is not conducive to improving the uniformity of the material network structure; if the particle size is too large, it will affect the optical properties of the PVA optical film and the subsequent iodine dyeing process of the polarizer, resulting in a decrease in the transmittance of the base film, an increase in the haze, and a deterioration in the hue and uniformity of the polarizer.

[0014] Furthermore, the mass proportion of carbon dots in the casting solution is 0.003%-0.15%, preferably 0.025%-0.075%. Too high a carbon dot content will cause excessive crosslinking inside the material, increase the modulus, and cause excessive tension in the downstream stretching process, which will make it easier to break the film; too low a carbon dot content will not form sufficient crosslinking and will not effectively improve the tensile properties of the material.

[0015] Furthermore, the polymerization degree of the PVA resin in the film casting solution is 1200-4000, preferably 1700-3000.

[0016] If the polymerization degree is too low, the physical cross-linking network stability of the prepared PVA molecular chain itself will be worse, the cross-linking effect of the carbon dots will be less obvious, and it will be less conducive to the improvement of tensile properties; if the polymerization degree is too high, it will cause excessive cross-linking and excessive tensile tension during the processing, which will cause breakage.

[0017] Furthermore, the alcoholysis degree of the PVA resin in the film casting stock solution is 90-99.9%, preferably 99-99.9%.

[0018] If the alcoholysis degree is too low, the hydrogen bond content of the prepared PVA molecular chain will be lower, the sites that can interact with carbon dots will be fewer, the cross-linking effect will be worse, the network stability will be worse, and it will be unfavorable for improving the tensile properties. In addition, if the alcoholysis degree is too low, the solubility will also deteriorate, and the optical properties of PVA will also deteriorate. The softening temperature of the prepared film in water is too low, which will have an adverse effect on the downstream production of polarizers.

[0019] Furthermore, the moisture content of the semi-finished product after pre-drying is 8-15%.

[0020] Too low a water content will cause excessive crystallization of the film during the cast molding and pre-drying stages, forming large and numerous crystals. These crystals will restrict the movement of the molecular chains due to the influence of steric hindrance, which is not conducive to the formation of the carbon dot cross-linked network, making the effect of improving the tensile properties worse. Too high a water content is not conducive to the subsequent heat treatment process, and is prone to problems such as dripping water and glycerin.

[0021] Furthermore, the additives in the film casting solution are plasticizers, surfactants and antioxidants;

[0022] The plasticizer is at least one of glycerol, diglycerol, polyglycerol, ethylene glycol and propylene glycol;

[0023] The plasticizer accounts for 3-5% by weight in the film casting stock solution;

[0024] The mass proportion of the surfactant in the film casting stock solution is 0.1-0.5‰.

[0025] Too much plasticizer and surfactant will precipitate, resulting in poor optical properties of the film.

[0026] Furthermore, the mass fraction of the solute in the film casting stock solution is 20-40%, preferably 30-35%.

[0027] Beneficial effects of the present invention:

[0028] From the perspective of formulation, the present invention, based on the nano effect of carbon dots and the large number of polar groups such as hydroxyl and carboxyl groups on its surface, can form micro-crosslinks with PVA hydroxyl groups, and form a double crosslinked network with the physical crosslinked network of PVA crystals to achieve a toughening effect. When stretched, the double network has different strengths, the weaker network breaks, dissipates a lot of energy, and the other network maintains the stability of the basic structure, greatly improving the elongation at break of the film. Optical film raw materials with certain characteristics are selected and the ratio is controlled to improve the PVA network and improve its stretchability, solving the problem of easy film breakage during polarizing film dyeing and stretching, and having little effect on other properties of the PVA optical film. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] Preparation of carbon dot solution:

[0032] Citric acid was selected as the carbon source, and citric acid was mixed with distilled water, and then ethylenediamine was added to the mixture to obtain a mixed solution, which was stirred with a glass rod until uniform. The concentration of citric acid in the mixed solution was 20 mmol / L, and the concentration of ethylenediamine was 20 mmol / L. The mixed solution was transferred to a polytetrafluoroethylene-lined autoclave, heated to 200°C, and kept at a constant temperature for 5 hours. After the reaction was completed, the reactants were naturally cooled to room temperature to obtain a brown-black transparent product. The obtained product was dialyzed with a dialysis bag for 48 hours, and freeze-dried after dialysis to obtain carbon dot powder with an average particle size of 10 nm.

[0033] Example 2

[0034] Preparation of carbon dot solution:

[0035] The difference from Example 1 is that the concentrations of citric acid and ethylenediamine in the mixed solution are increased to 80 mmol / L, the concentration of ethylenediamine is increased to 80 mmol / L, the constant temperature time is adjusted to 15 h, and the other steps are the same as Example 1. The average particle size of the carbon dots is measured to be 16 nm.

[0036] Example 3

[0037] Preparation of carbon dot solution:

[0038] The difference from Example 1 is that the concentrations of citric acid and ethylenediamine in the mixed solution are increased to 240 mmol / L, the concentration of ethylenediamine is increased to 240 mmol / L, the constant temperature time is adjusted to 45 h, and the other steps are the same as Example 1. The average particle size of the carbon dots is measured to be 25 nm.

[0039] Example 4

[0040] Preparation of PVA optical film:

[0041] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 2.5 carbon dot powder (prepared in Example 2, with an average particle size of 16nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment to reduce the water content to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0042] Example 5

[0043] Preparation of PVA optical film:

[0044] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 0.5 carbon dot powder (prepared in Example 2, with an average particle size of 16nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0045] Example 6

[0046] Preparation of PVA optical film:

[0047] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 7.5 carbon dot powder (prepared in Example 2, with an average particle size of 16nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment to reduce the water content to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0048] Example 7

[0049] Preparation of PVA optical film:

[0050] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 2.5 carbon dot powder (prepared in Example 1, with an average particle size of 10nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0051] Example 8

[0052] Preparation of PVA optical film:

[0053] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 2.5 carbon dot powder (prepared in Example 3, with an average particle size of 25nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0054] Example 9

[0055] Preparation of PVA optical film:

[0056] 3111g PVA resin (polymerization degree 1700, alcoholysis degree 99%), 2.5 carbon dot powder (prepared in Example 2, with an average particle size of 16nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0057] Example 10

[0058] Preparation of PVA optical film:

[0059] 3111g PVA resin (polymerization degree 3000, alcoholysis degree 99%), 2.5 carbon dot powder (prepared in Example 2, with an average particle size of 16nm), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0060] Comparative Example 1

[0061] Preparation of PVA optical film:

[0062] 3111g PVA resin (polymerization degree 2400, alcoholysis degree 99%), 8g sodium dodecylbenzene sulfonate, 5g sodium fatty alcohol polyoxyethylene ether carboxylate, 373g injection-grade glycerol and 3g sodium thiosulfate were added to a high-pressure reactor, and 6500mL deionized water was added as a solvent in the high-pressure reactor. The mixture was stirred at 150°C and 0.4MPa for 6h to obtain a casting solution with a solute mass ratio of 35%. The formed casting solution was degassed and filtered by an extruder and then extruded from a die. After cast molding, it entered a drying roller for pre-drying. The water content after pre-drying was 10%. It then entered an oven for heat treatment, and the water content was reduced to 2%. Finally, the PVA optical film was rolled up to obtain a thickness of 30μm.

[0063] The performance of the PVA optical films prepared in Examples 4 to 10 and Comparative Example 1 was tested, and the results are shown in Table 1.

[0064] The tensile properties of PVA optical films were tested with reference to GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Test conditions for films and sheets. The average elongation at break was obtained by taking the average value of the three samples.

[0065] The optical performance test of PVA optical film was carried out with reference to "GB / T 2410-2008 Determination of light transmittance and haze of transparent plastics" to obtain the light transmittance and haze data of the film.

[0066] The PVA optical films prepared in Examples 4-10 and Comparative Example 1 were respectively immersed in deionized water at 27°C for 2.5 min, then dyed in a solution containing 0.335 g / L iodine, 12 g / L potassium iodide and 0.6 g / L boric acid for 4 min, taken out and washed in a solution containing 32 g / L boric acid (35°C) for 1 min, then stretched while dyeing in a solution containing 20 g / L potassium iodide and 32 g / L boric acid (53°C), stretched to 5.5 times, and finally color-corrected in a solution containing 34 g / L potassium iodide and 6 g / L boric acid (25°C), and finally dried at 55°C, TAC films were attached to the upper and lower surfaces of the dried film, a protective film was attached to the outside of the upper surface TAC film, a pressure-sensitive adhesive was coated on the outside of the lower surface TAC film, a release film was attached to the outside of the pressure-sensitive adhesive, and a polarizer was obtained after drying. The test was carried out with reference to the standard "GB / T 25275-2010 Test method for optical properties and weather resistance of polarizers for liquid crystal displays (LCD)" to obtain the polarization degree and single transmittance data of the polarizer.

[0067] Table 1

[0068]

[0069]

[0070] As can be seen from Table 1, the optical film prepared in Example 4 has a higher elongation at break than the optical film without carbon dots added in Comparative Example 1, indicating that carbon dots can effectively improve the tensile properties of the optical film. In Examples 4-8, the proportion of carbon dots and the different particle sizes will have different degrees of influence on the tensile properties of the material. Too large a particle size of carbon dots and excessive addition will cause a decrease in optical properties, while too small a particle size of carbon dots and too little addition will reduce the tensile properties. Compared with Example 1, the polymerization degree of the PVA resin was adjusted in Examples 9 and 10, and the tensile properties of Examples 9 and 10 were not as good as those of Example 4. According to the polarization degree test data of the prepared polarizer, the addition of carbon dots has little effect on the polarization degree.

[0071] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a PVA optical film with excellent stretchability, characterized in that: The following steps are involved: (1) dissolving PVA resin and additives in a solvent and adding carbon dots to prepare a film casting solution; (2) mixing the film casting stock solution uniformly, extruding and degassing it, and casting it through a die head to obtain a semi-finished product; (3) The semi-finished product is pre-dried by a drying guide roller and then placed in a heat treatment oven for drying and shaping to obtain a PVA optical film.

2. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The thickness of the PVA optical film is less than 45 μm.

3. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The average particle size of the carbon dots is 5nm-50nm.

4. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The average particle size of the carbon dots is 10nm-25nm.

5. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The mass proportion of carbon dots in the film casting solution is 0.003%-0.15%.

6. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The mass proportion of carbon dots in the film casting stock solution is 0.025%-0.075%.

7. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The polymerization degree of the PVA resin in the film casting stock solution is 1200-4000.

8. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The polymerization degree of the PVA resin in the film casting stock solution is 1700-3000.

9. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The mass fraction of the solute in the film casting stock solution is 20-40%.

10. The method for preparing a PVA optical film with excellent stretchability according to claim 1, characterized in that: The mass fraction of the solute in the film casting stock solution is 25-35%.

Citation Information

Cited By

  • Flexible sensor with photoresponse and preparation method thereof

    CN120028299A