Biodegradable composite foam and preparation method thereof

By using borate crosslinking agent, biomass polyelectrolyte and SiO2 aerogel, combined with polyvinyl alcohol and emulsifier, pulp foam with excellent mechanical properties and flame retardant properties is prepared, which solves the insufficient performance of the pulp foam material. Problem, environmental protection, simplified process and degradability are achieved.

CN118909302APending Publication Date: 2024-11-08QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960255.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The mechanical properties and flame retardant properties of existing pulp foam materials are insufficient and the production process is complex, resulting in a decrease in performance in humid environments, and there are problems of environmental protection and low resource utilization efficiency.

Method used

Boric acid or borate as crosslinking agent, combined with biomass polyelectrolyte and SiO2 aerogel, pulp suspension is formed by mechanical stirring and ultrasonic treatment, polyvinyl alcohol and emulsifier are added, and the preparation is excellent after freezing and vacuum drying. Composite foam with mechanical properties and flame retardant properties.

Benefits of technology

It improves the mechanical properties and flame retardant properties of pulp foam, broadens its application areas, simplifies production processes, reduces environmental threats, and achieves good performance maintenance and degradability in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909302A_ABST
    Figure CN118909302A_ABST
Patent Text Reader

Abstract

The invention discloses biodegradable composite foam and a preparation method thereof, and relates to the technical field of paper pulp foams, and the technical scheme is as follows: firstly, adding paper pulp into deionized water, mechanically stirring, and uniformly dispersing through ultrasonic treatment to form a suspension; dissolving polyvinyl alcohol in heated deionized water, and cooling for later use; mixing the paper pulp suspension with a polyvinyl alcohol solution, adding a flame-retardant cross-linking agent, adjusting the pH value, adding biomass polyelectrolyte and SiO2 aerogel, and stirring to obtain a mixed solution; then adding a foaming agent and an emulsifying agent to form foam, filtering, freezing and shaping, soaking and drying to obtain the composite foam material. The borate is used as a cross-linking agent, so that the mechanical properties of the polyvinyl alcohol and the paper pulp fibers are improved, the flame-retardant self-extinguishing performance is also endowed, and the performance of the flame-retardant self-extinguishing paper pulp in a humid environment is improved. By adding the biomass polyelectrolyte, the flame retardance, the environmental protection property and the degradability are enhanced, the preparation process is simple and environmentally friendly, and the industrial application potential is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pulp foam, and in particular to a biodegradable composite foam and a preparation method thereof. Background Art

[0002] Foam materials are solid materials formed by a large amount of gas filling many connected or unconnected micropores. Foam materials have excellent special properties such as light weight, low thermal conductivity, cushioning and shock absorption, and high adsorption due to their low density, high porosity, and high specific surface area. They have become a research hotspot in the field of new materials. However, most foam materials are polymer foams made of non-degradable petroleum-based materials, such as polyurethane foam, polyvinyl chloride foam, polyethylene foam, etc. However, their molecular structure determines their non-degradable characteristics, which poses a threat to the environment and resources. Therefore, the development of degradable and green foam materials to replace petroleum-based foam materials is an emerging direction in the field of foam materials. Cellulose is the most abundant natural polymer on earth and is widely present in plant cell walls. Cellulose-based foam materials are one of the research hotspots in the field of foam materials. In addition to the excellent properties mentioned above, they are also biodegradable, and the cellulose surface contains a large number of hydroxyl groups, which is convenient for further modification.

[0003] Pulp is a fibrous material made from plant fibers through different processing methods. The main component of the fiber in pulp is cellulose. Pulp has excellent biodegradability and renewability, and the surface of pulp fibers is rich in hydroxyl groups and is easy to modify. Pulp foam materials can be obtained using foam molding technology, which have good thermal insulation and sound absorption properties. However, most of the current pulp foam materials use foaming agents to obtain porous structures under the action of mechanical stirring. This method removes the rich lignin between fiber cells, resulting in poor flame retardancy and mechanical properties.

[0004] In order to solve the problem of poor mechanical properties of pulp foam, researchers have enhanced foam materials by adding various inorganic and organic fillers. Invention patent CN106835805A discloses "a pulp foam material reinforced with nanocellulose and a preparation method thereof". The invention uses nanocellulose to enhance the pore structure and obtains a pulp foam material with good mechanical properties, simple process and greenness by controlling the foaming process. Although this technology improves the compressive strength of pulp foam, it is still insufficient compared with other foam materials, and the patent does not study the flame retardant properties of the foam. Invention patent CN116903921A discloses "a pulp foam material and a preparation method thereof". The invention modifies sepiolite powder and adds it to the pulp solution, which not only avoids sepiolite agglomeration, but also promotes the combination with other components, improves the stability and uniformity of the pores, improves the mechanical properties, and reduces the thermal conductivity, and can maintain good mechanical properties even in a humid state. However, this technology requires modification and post-processing, and there are problems such as complex process and long production cycle.

[0005] Therefore, developing a pulp foam with excellent flame retardant and mechanical properties, simple production process, environmental protection and recyclability is one of the problems that need to be solved urgently. Summary of the invention

[0006] In order to achieve the above-mentioned invention objectives and address the above-mentioned technical problems,

[0007] The present invention provides a method for preparing a biodegradable composite foam, the method comprising the following steps:

[0008] S1: adding pulp into deionized water and dispersing the pulp under mechanical stirring to form a pulp suspension, and ultrasonically treating the pulp suspension to achieve uniform dispersion;

[0009] S2: adding polyvinyl alcohol to deionized water and heating and stirring to form a polyvinyl alcohol solution, and then cooling the polyvinyl alcohol solution to room temperature for later use;

[0010] S3: mixing the pulp suspension obtained in step S1 with the polyvinyl alcohol solution obtained in step S2, adding a flame retardant crosslinking agent, setting the temperature and adjusting the pH value of the solution, adding biomass polyelectrolyte and SiO2 aerogel after continuing to stir, and continuing to stir and mix to obtain a mixed solution.

[0011] S4 adds a foaming agent and an emulsifier to the mixed solution of step S3, and stirs evenly to obtain mixed foam;

[0012] S5: pouring the mixed foam obtained in step S4 into a gauze container for filtration, and then pouring it into a mold for freezing and shaping. The frozen foam is immersed in a saturated calcium chloride solution, and finally vacuum dried to obtain a composite foam.

[0013] Preferably, the flame retardant crosslinking agent is selected from borate or boric acid, the concentration thereof is 0.01-0.05 g / ml, and the amount thereof is 0.5%-1.5% of the total mass of the pulp and polyvinyl alcohol, and the pulp is bleached pulp or log pulp.

[0014] Preferably, the preparation steps of the biomass polyelectrolyte flame retardant are as follows:

[0015] A1 was added dropwise to 2-5 ml of glacial acetic acid solution in 100 ml of deionized water, and then 2-5 g of chitosan powder was added, and the mixture was stirred at 50°C and 500-1500 rpm for 2 h to dissolve the chitosan, thereby obtaining solution A;

[0016] A2 was added to 100 mL of deionized water, and 1-2.5 g of sodium alginate powder was added. The mixture was stirred at 50°C and 500-1500 rpm for 2 h and dissolved to obtain solution B.

[0017] A3: Mix solution A and solution B, add 2-5 g of phytic acid solution with a mass concentration of 50% to the mixed solution, and stir at room temperature for 0.5 h to obtain a polyelectrolyte solution;

[0018] A4: drying the polyelectrolyte solution in a vacuum drying oven at 50° C. to constant weight, and grinding the solution into powder to obtain a biomass polyelectrolyte flame retardant.

[0019] Preferably, the borate is sodium tetraborate decahydrate, sodium metaborate or sodium polyborate.

[0020] Preferably, the mass concentration of the pulp suspension in step S1 is 2%-5%; and the ultrasonic treatment time is 30-60 minutes.

[0021] Preferably, in step S2, the weight ratio of polyvinyl alcohol to deionized water is 1:(15-30), the temperature of heating and stirring is 90-100° C., the time of heating and stirring is 1-3 h; and the time of continued stirring is 30 min.

[0022] Preferably, in step S3, the mass ratio of pulp to polyvinyl alcohol is 1:9-3:7; the amount of biomass polyelectrolyte flame retardant added is 20%-40% of the total mass of pulp and polyvinyl alcohol; 2 The amount of aerogel added is 0%-20% of the total mass of pulp and polyvinyl alcohol; the temperature is set at 30-50°C; the pH value is adjusted to 10; the stirring speed is 2500-4000rpm, and the stirring and mixing time is 1-2h.

[0023] Preferably, in step S4, the foaming agent is sodium dodecyl sulfate or Tween 80, and the addition amount is 0.4-0.8% of the mass of the mixed solution; the emulsifier is OP-10 or polyacrylamide, and the addition amount is 1-3% of the volume of the mixed solution. The stirring time is 3-5 minutes, and the stirring speed is 2500-4000rpm.

[0024] Preferably, in step S5, the aperture of the gauze container is 100 mesh; the freezing temperature is -20°C, the freezing time is 6-24h; the soaking time is 12h; the drying temperature is 60°C, and the drying time is 12h.

[0025] The present invention also provides a biodegradable composite foam, which is prepared by the above-mentioned preparation method.

[0026] The technical solution provided by the present invention brings beneficial effects:

[0027] 1. Boric acid or borate is used as a crosslinking agent, which can not only crosslink pulp fibers, but also serve as an excellent crosslinking agent for polyvinyl alcohol to obtain a double crosslinked network. The crosslinked polyvinyl alcohol forms an interpenetrating network with the pulp fiber network, which can effectively improve the mechanical properties of pulp foam. At the same time, polyvinyl alcohol crosslinked with boric acid can improve the water solubility and solubility of PVA, thereby giving pulp foam the ability to maintain good performance in a humid environment.

[0028] 2. The present invention uses borate as a crosslinking agent, biomass polyelectrolyte and SiO 2 Aerogel is a flame retardant that not only gives pulp foam excellent mechanical properties, but also excellent flame retardant and self-extinguishing properties. The use of borate crosslinking agent enables the foam to have both good mechanical properties and flame retardant properties, broadening the application field of pulp foam and bringing more application value to pulp foam.

[0029] 3. The present invention uses polyvinyl alcohol as a reinforcing material, which has excellent biodegradability, so that pulp foam can achieve further breakthroughs in the fields of recycling and degradation, and can be used for the preparation of non-disposable foam.

[0030] 4. The preparation scheme provided by the present invention is simple, green and environmentally friendly, has little threat to the environment, is easy to operate, and has industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 are electron microscope images of Example 1 and Comparative Example 1 of the present invention, wherein a is an electron microscope image of Example 1, b is an electron microscope image of Comparative Example 1, c is an electron microscope enlarged image of Example 1, and d is an electron microscope enlarged image of Comparative Example 1;

[0032] Figure 2are photos of samples of the present invention, wherein a is a photo of Example 1, b is a photo of Comparative Example 1, c is a photo of Example 2, and d is a photo of Example 3;

[0033] Figure 3 The electron microscope images of the cell structure of Example 4 of the present invention, wherein a is the cell structure of Example 4, and b is an enlarged view of Example 4;

[0034] Figure 4 This is the cell structure of Comparative Example 3 of the present invention;

[0035] Figure 5 The sample photos of Example 5 and Comparative Example 2 of the present invention are shown below;

[0036] Figure 6 The cone calorimeter photos after combustion of comparative examples 1 and 2 of Example 5 of the present invention are shown;

[0037] Figure 7 This is a photo of Comparative Example 1 of the present invention after moisture absorption;

[0038] Figure 8 This is a photograph of Example 4 of the present invention after moisture absorption. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0040] Example 1

[0041] S1: adding pulp into deionized water and dispersing the pulp under mechanical stirring to form a pulp suspension with a mass concentration of 3%, and subjecting the pulp suspension to ultrasonic treatment for 30 minutes to achieve uniform dispersion;

[0042] S2: adding polyvinyl alcohol to deionized water and heating to 95°C, stirring for 2 hours to form a polyvinyl alcohol solution, wherein the weight ratio of polyvinyl alcohol to deionized water is 1:20, and then continuing to stir the polyvinyl alcohol solution for 30 minutes and cooling to room temperature for later use;

[0043] S3: Mix the pulp suspension obtained in step S1 with the polyvinyl alcohol solution obtained in step S2, wherein the mass ratio of pulp to polyvinyl alcohol is 9:1, and then add sodium borate, a flame retardant crosslinking agent, with a concentration of 0.05 g / ml, in an amount of 1% of the total mass of the pulp and polyvinyl alcohol, set the temperature to 40°C and adjust the pH value of the solution to 10, continue stirring, and then add biomass polyelectrolyte and SiO 2 aerogel, and continue to stir and mix to obtain a mixed solution, wherein the biomass polyelectrolyte flame retardant is added in an amount of 40% of the total mass of the pulp and the polyvinyl alcohol, and the SiO2 The amount of aerogel added was 0% of the total mass of pulp and polyvinyl alcohol; the stirring speed was 2500 rpm, and the stirring mixing time was 1 h;

[0044] S4: adding sodium lauryl sulfate as a foaming agent to the mixed solution of step S3 in an amount of 0.5% of the mass of the mixed solution and OP-10 as an emulsifier in an amount of 2% of the volume of the mixed solution, stirring evenly to obtain mixed foam, the stirring time is 3 minutes, and the stirring speed is 2500 rpm;

[0045] S5: pouring the mixed foam obtained in step S4 into a gauze container with a pore size of 100 meshes for filtration, and then pouring it into a mold for freezing and shaping at -20°C for 12 hours, soaking the frozen foam in a saturated calcium chloride solution for 12 hours, and finally vacuum drying at 60°C for 12 hours to obtain a polyvinyl alcohol pulp foam composite material;

[0046] The preparation steps of the biomass polyelectrolyte flame retardant are as follows:

[0047] A1 was added dropwise with 2 ml of glacial acetic acid solution to 100 ml of deionized water, and then 2 g of chitosan powder was added, and the mixture was stirred at 50°C and 1000 rpm for 2 h to dissolve the chitosan, thereby obtaining solution A;

[0048] A2 was dissolved in 100 mL of deionized water by adding 1.4 g of sodium alginate powder, and stirred at 50 °C and 1000 rpm for 2 h to obtain solution B.

[0049] A3: Mix solution A and solution B, add 2.8 g of phytic acid solution with a mass concentration of 50% to the mixed solution, and stir at room temperature for 0.5 h to obtain a polyelectrolyte solution;

[0050] A4: drying the polyelectrolyte solution in a vacuum drying oven at 50° C. to constant weight, and grinding the solution into powder to obtain a biomass polyelectrolyte flame retardant.

[0051] Embodiment 2-4

[0052] The preparation was carried out in the same manner as in Example 1, except that the ingredients and process parameters were adjusted according to Table 1.

[0053] Embodiment 5-9

[0054] The biomass polyelectrolyte flame retardant was prepared according to the same preparation method as in Example 1, and the ingredients and process parameters were adjusted according to Table 1. The difference was that the preparation steps of the biomass polyelectrolyte flame retardant were as follows:

[0055] A1 was added dropwise with 2 ml of glacial acetic acid solution to 100 ml of deionized water, and then 5 g of chitosan powder was added, and the mixture was stirred at 50°C and 1000 rpm for 2 h to dissolve the chitosan, thereby obtaining solution A;

[0056] A2 was dissolved in 100 mL of deionized water by adding 2.5 g of sodium alginate powder, and stirred at 50 °C and 1000 rpm for 2 h to obtain solution B.

[0057] A3: Mix solution A and solution B, add 4 g of phytic acid solution with a mass concentration of 50% to the mixed solution, and stir at room temperature for 0.5 h to obtain a polyelectrolyte solution;

[0058] A4: drying the polyelectrolyte solution in a vacuum drying oven at 50° C. to constant weight, and grinding the solution into powder to obtain a biomass polyelectrolyte flame retardant.

[0059] Comparative Examples 1-3

[0060] The preparation was carried out in the same manner as in Example 1, except that the ingredients and process parameters were adjusted according to Table 1.

[0061] Table 1 Formula table of embodiments and comparative examples

[0062]

[0063]

[0064] Table 2 Test data table of embodiments and comparative examples

[0065]

[0066] Example 1 exhibits a relatively low density (0.035 g / cm 3 ), which shows that the lightweight treatment effect of the material is good, better than that of comparative example 1 (0.032g / cm 3 ), and is much lower than Comparative Examples 2 and 3, which supports the superiority of the material structure provided by the invention.

[0067] The compressive strengths of Examples 1-9 are generally higher than those of the comparative example, especially Example 5 (947 kPa), indicating that the mechanical properties of the material are significantly improved by optimizing the use of borate and biomass polyelectrolyte.

[0068] The limiting oxygen index of all examples is higher than 30%, and the afterflame time and afterglow time are less than 1 second, indicating that these materials have excellent flame retardancy, which is much better than the comparative example (limiting oxygen index is 17%-26%), which highlights the advantages of borate and biomass polyelectrolyte and SiO 2 Effectiveness of aerogels as flame retardants.

[0069] All examples achieve a V-0 flame retardant rating, while Comparative Examples 1 and 2 do not. The porosity of the examples is moderate, which helps to maintain good flame retardant properties without sacrificing too much physical properties.

[0070] By comparing the data of the embodiment with the comparative example, it can be seen that:

[0071] The use of borate as a cross-linking agent not only enhances the bonding between polyvinyl alcohol and pulp fibers, but also improves the mechanical strength and flame retardancy of the overall composite material, which is completely consistent with the purpose of the invention.

[0072] The high proportion of biomass polyelectrolyte (40%) effectively improves the flame retardant performance, which is consistent with its designed use. The low density and high porosity of the material in the embodiment show that the material has good insulation and lightweight properties and is suitable for a wide range of applications.

[0073] from Figure 1 It can be seen from the figure that after adding PVA to the system, the surface of the pulp fiber is coated with PVA, and the maximum compression strength increases when the density difference is not large. It can also be seen from the photo that after mixing with PVA, it becomes denser.

[0074] from Figure 2 It can also be seen from the photos of Examples 1-3 that as the PVA content increases, the cells become denser, and although the density increases slightly, the strength is greatly improved.

[0075] From above Figure 3 and 4 As can be seen from the two figures, when PVA is dominant in the system, the pore structure changes, and the pulp fibers are now wrapped in PVA, and the pulp fibers can be shown after magnification. 2 The number of aerogel parts exceeds 20, which is 30. It can be seen that SiO 2 The amount of aerogel affects the open porosity of the material and the density also increases.

[0076] As can be seen from Figure 5, when the ratio of pulp to PVA is the same, the sample without adding flame retardant will shrink, which also leads to an increase in its density.

[0077] from Figure 6 From the cone calorimeter photos after combustion, it can be seen that the pure pulp is almost burned out without much residue; the pulp / PVA30 / 70 sample without flame retardant also has a thin layer left after burning, while the sample with flame retardant can still maintain its intact shape after burning.

[0078] from Figure 7 , Figure 8It can be seen that after absorbing moisture, the comparative example 1 is cracked, incomplete, and has no strength, and cannot be used. Because it has been damaged, it is no longer intact after drying; after absorbing moisture, the example 4 can maintain a certain strength and can be bent and pressed without being damaged. When the water in it dries, it can still maintain the original hard high strength and can be recycled.

[0079] In general, the material preparation method of the present invention can effectively prepare a polyvinyl alcohol pulp foam composite material with excellent mechanical properties, high flame retardant properties and good environmental adaptability. These properties make the material have a wide range of application prospects in the construction, packaging and automotive industries.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a biodegradable composite foam, characterized in that: The method comprises the following steps: S1: adding pulp into deionized water and dispersing the pulp under mechanical stirring to form a pulp suspension, and ultrasonically treating the pulp suspension to achieve uniform dispersion; S2: adding polyvinyl alcohol to deionized water and heating and stirring to form a polyvinyl alcohol solution, and then cooling the polyvinyl alcohol solution to room temperature for later use; S3: mixing the pulp suspension obtained in step S1 with the polyvinyl alcohol solution obtained in step S2, adding a flame retardant crosslinking agent, setting the temperature and adjusting the pH value of the solution, adding biomass polyelectrolyte and SiO2 aerogel after continuing to stir, and continuing to stir and mix to obtain a mixed solution; S4 adds a foaming agent and an emulsifier to the mixed solution of step S3, and stirs evenly to obtain mixed foam; S5: pouring the mixed foam obtained in step S4 into a gauze container for filtration, and then pouring it into a mold for freezing and shaping. The frozen foam is immersed in a saturated calcium chloride solution, and finally vacuum dried to obtain a composite foam.

2. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: The flame retardant crosslinking agent is selected from borate or boric acid, and its concentration is 0.01-0.05 g / ml. Its usage is 0.5%-1.5% of the total mass of the pulp and polyvinyl alcohol. The pulp is bleached pulp or log pulp.

3. The method for preparing the biodegradable composite foam according to claim 2, characterized in that: The preparation steps of the biomass polyelectrolyte flame retardant are as follows: A1 is added dropwise to 100 ml of deionized water with 2-5 ml of glacial acetic acid solution, and then 2-5 g of chitosan powder is added, and the mixture is stirred at 50°C and 500-1500 rpm to dissolve the chitosan to obtain solution A; A2 was added to 100 mL of deionized water, and 1-2.5 g of sodium alginate powder was added. The mixture was stirred and dissolved at 50°C and 500-1500 rpm to obtain solution B. A3: Mix solution A and solution B, add 2-5 g of phytic acid solution with a mass concentration of 50% to the mixed solution, and stir evenly at room temperature to obtain a polyelectrolyte solution; A4: drying the polyelectrolyte solution in a vacuum drying oven at 50° C. to constant weight, and grinding the solution into powder to obtain a biomass polyelectrolyte flame retardant.

4. The method for preparing the biodegradable composite foam according to claim 2, characterized in that: The borate is sodium tetraborate decahydrate, sodium metaborate or sodium polyborate.

5. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: The mass concentration of the pulp suspension in step S1 is 2%-5%; and the ultrasonic treatment time is 30-60 minutes.

6. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: In the step S2, the weight ratio of polyvinyl alcohol to deionized water is 1:(15-30), the heating and stirring temperature is 90-100°C, the heating and stirring time is 1-3h; and the continued stirring time is 30min.

7. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: In the step S3, the mass ratio of pulp to polyvinyl alcohol is 1:9-3:7; the amount of the biomass polyelectrolyte flame retardant added is 20%-40% of the total mass of the pulp and polyvinyl alcohol; the amount of the SiO2 aerogel added is 0%-20% of the total mass of the pulp and polyvinyl alcohol; the temperature is set to 30-50°C; the pH value is adjusted to 10; the stirring speed is 2500-4000rpm, and the stirring and mixing time is 1-2h.

8. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: In step S4, the foaming agent is sodium dodecyl sulfate or Tween 80, and the addition amount is 0.4-0.8% of the mass of the mixed solution; the emulsifier is OP-10 or polyacrylamide, and the addition amount is 1-3% of the volume of the mixed solution. The stirring time is 3-5 minutes, and the stirring speed is 2500-4000rpm.

9. The method for preparing the biodegradable composite foam according to claim 1, characterized in that: In step S5, the aperture of the gauze container is 100 meshes; the freezing temperature is -20°C, the freezing time is 6-24 hours; and the soaking time is 12 hours.

10. A biodegradable composite foam, characterized in that: Prepared by the method of any one of claims 1 to 9.