Preparation method of modified quartz fiber and application of modified quartz fiber in composite material

Through the preparation method of modified quartz fiber, dilute nitric acid hydroxylation and hydrogen-containing silane reaction form covalent bonds, combined with acetone cleaning and vacuum molding technology, the problem of degradation of mechanical properties of quartz fiber/silicone composites at high temperatures is solved. It has achieved high strength and heat resistance of the material, and is suitable for applications such as high-temperature radomes.

CN118909308APending Publication Date: 2024-11-08HARBIN INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410959961.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The problem of degradation of mechanical properties of quartz fiber/silica resin composites at high temperatures is mainly due to the poor temperature resistance of quartz fiber surface treatment agents, which leads to a reduction in the interface force between quartz fiber and silicone.

Method used

The preparation method of modified quartz fibers includes hydroxylation of quartz fibers in dilute nitric acid, and covalent bonds are formed by reaction between hydrogen-containing silane and catalyst, followed by hydrolysis-condensation reaction in dilute hydrochloric acid to improve quartz fibers and silicon. The binding force of the resin, combined with acetone cleaning and vacuum molding technology, produces high-strength modified quartz fiber/silicon composites.

Benefits of technology

The room temperature and high temperature mechanical properties of composite materials are significantly improved, the binding force between quartz fiber and silicone resin is enhanced, and the material is not easy to decompose at high temperatures, and is suitable for applications such as high-temperature resistant radomes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909308A_ABST
    Figure CN118909308A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of modified quartz fibers and application of the modified quartz fibers in a composite material, and belongs to the technical field of quartz fiber reinforced silicon resin composites.The method comprises the steps that quartz fiber cloth is repeatedly refluxed, cleaned and dried with acetone, and an impregnating compound on the surface of the quartz fibers is removed; placing the cleaned quartz fibers in dilute nitric acid for reaction, and carrying out hydroxylation on the quartz fibers; the preparation method comprises the following steps: putting hydroxylated quartz fibers into tetrahydrofuran, adding hydrogen-containing silane and a catalyst, carrying out a heating reaction, slowly dropwise adding a diluted hydrochloric acid solution into a reaction system, and after the reaction is finished, washing and drying to obtain modified quartz fibers; and compounding the modified quartz fiber and hydroxyl silicone resin, and performing vacuum compression molding to prepare the modified quartz fiber / silicone resin composite material. The preparation method disclosed by the invention is simple to operate, and the mechanical property, especially the high-temperature mechanical property, of the quartz fiber reinforced silicon resin can be improved while the excellent high-temperature resistance of the quartz fiber reinforced silicon resin is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of quartz fiber reinforced silicone resin composite materials, and specifically relates to a preparation method of modified quartz fiber and application of the modified quartz fiber in high-temperature resistant and high-strength quartz fiber / silicone resin composite materials. Background Art

[0002] Quartz fiber / silicone resin composite material is a functional composite material formed by mixing quartz fiber and silicone resin matrix material in a certain proportion. Quartz fiber has the characteristics of heat resistance, high specific strength and specific modulus. Quartz fiber / silicone resin composite material has low dielectric constant and dielectric loss, and is not easily affected by temperature and frequency. It is one of the commonly used materials for high-temperature radar antenna covers, antenna windows and other wave-transmitting components. In the production of quartz fiber, surface treatment agents are needed to improve the quality of quartz fiber. Currently, the commonly used surface treatment agents are mainly epoxy and epoxy K. The surface treatment agent can improve the interface bonding force between quartz fiber and matrix resin, which is beneficial to improve the mechanical properties of the composite material.

[0003] Due to its excellent heat resistance, the composite materials prepared by silicone resin are stable at room temperature and can reach 500°C in a short time. However, the main component of quartz fiber surface treatment agent is epoxy resin, which has poor temperature resistance and begins to decompose at 300°C. The decomposition of the surface treatment agent will lead to a decrease in the interfacial force between quartz fiber and silicone resin, and a significant decrease in the high-temperature mechanical properties of quartz fiber / silicone resin. Summary of the invention

[0004] In order to solve the problem that the high-temperature mechanical properties of a quartz fiber / silicone resin composite material decrease due to high-temperature decomposition of a quartz fiber sizing agent, the present invention provides a preparation method of a modified quartz fiber and an application of the modified quartz fiber in a high-temperature resistant and high-strength quartz fiber / silicone resin composite material, so as to improve the mechanical properties and high-temperature mechanical property retention rate of the quartz fiber / silicone resin composite material.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing modified quartz fiber comprises the following steps:

[0007] Step 1: Arrange the cut quartz fiber in acetone for reflux, wash it with acetone 2-3 times, vacuum dry it, repeat reflux-wash-dry three times to obtain the cleaned quartz fiber with the impregnant removed, then place it in a dilute nitric acid solution for reaction, wash it with tetrahydrofuran after the reaction is completed, and vacuum dry it to obtain hydroxylated quartz fiber;

[0008] Step 2: placing the hydroxylated quartz fiber in tetrahydrofuran, then adding hydrosilane and a catalyst thereto and heating for reaction, and naturally cooling to room temperature after the reaction is completed;

[0009] Step 3: slowly drop a dilute hydrochloric acid solution into the reaction system of step 2 and heat to react. After the reaction is completed, wash with anhydrous ethanol and dry to obtain modified quartz fiber.

[0010] Furthermore, in step 1, the mass ratio of quartz fiber to dilute nitric acid solution is 100:50-200, the concentration of dilute nitric acid solution is 0.5-2.0 mol / L, the reaction temperature is 60-90° C., and the reaction time is 6-12 hours.

[0011] Furthermore, the mass ratio of the quartz fiber to the acetone for reflux is 100:50-200, the reflux temperature is 45-60° C., and the reflux time is 8-12 hours.

[0012] Furthermore, in step 1, the vacuum degree of vacuum drying is -0.1 to -0.06 MPa, the temperature is 30 to 50° C., and the drying time is 4 to 8 hours.

[0013] Furthermore, in step 2, the mass ratio of the quartz fiber to tetrahydrofuran is 100:150-300; the mass ratio of the quartz fiber to the hydrogen-containing silane is 100:2-10; the mass ratio of the catalyst to the hydrogen-containing silane is 0.01-0.5:100, the reaction temperature is 60-80°C, and the reaction time is 2-8 hours.

[0014] Furthermore, the hydrogen-containing silane is a combination of methylphenylsilane, dimethylsilane and phenylsilane, and the mass ratio of the three is 5-20:5-15:3-20; the catalyst includes a combination of one or more of chloroplatinic acid and Karstedt catalyst.

[0015] Furthermore, in step three, the concentration of the dilute hydrochloric acid solution is 0.02-0.05 mol / L, the mass ratio of the dilute hydrochloric acid solution to the quartz fiber is 5-15:100, the dripping rate is 2-5 mL / min, the reaction temperature is 50-80° C., and the reaction time is 4-12 hours.

[0016] An application of the modified quartz fiber prepared by the preparation method includes the following steps: heating the hydroxy silicone resin at 60-80°C for 2-4 hours, coating the melted hydroxy silicone resin on a modified quartz fiber cloth to obtain a prepreg, wherein the silicone resin content in the prepreg is 30%-45%. The prepreg is vacuum molded and cured at high temperature to obtain a high-strength modified quartz fiber / silicone resin composite material.

[0017] Furthermore, the hydroxy silicone resin has a hydroxyl value content of 3-8%, a phenyl content of 25%-50%, a molar ratio of organic groups to silicon atoms of 1.1-1.25:1, and a resin softening point of 50-60°C.

[0018] Furthermore, the vacuum degree of vacuum compression molding is ≤0.1MPa, and the curing system is heating at 120°C for 1h, then pressurizing to 10-20MPa, keeping the pressure constant, heating at 150°C for 1h, 200°C for 2h, and 250°C for 4h, cooling to room temperature and demolding to obtain a modified quartz fiber / silicone resin composite material.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The present invention first uses an acetone solution to clean the quartz fiber cloth, which can better remove the wetting agent with poor temperature resistance on the surface of the quartz fiber; then the quartz fiber is placed in dilute nitric acid for reaction. The nitric acid can react with the silicon dioxide of the quartz fiber to generate more silanol groups on the surface of the quartz fiber, which is more conducive to the next step of modification;

[0021] (2) Hydrogen-containing silane reacts with the hydroxyl groups on the surface of quartz fiber to form a covalent bond. The high reaction activity can improve the modification efficiency of quartz fiber. Hydrogen-containing silane undergoes a hydrolysis-condensation reaction under the catalysis of dilute hydrochloric acid to further modify the quartz fiber, thereby improving the modification efficiency and the utilization rate of hydrogen-containing silane. The schematic diagram of the reaction principle is shown in FIG. Figure 2 As shown;

[0022] (3) Silane-modified quartz fiber can better improve the bonding strength between quartz fiber and silicone resin matrix, thereby improving the room temperature mechanical properties of the composite material. At the same time, silane-modified quartz fiber has good heat resistance and is not easy to decompose at high temperature, which is beneficial to improving the high temperature mechanical properties of the composite material.

[0023] (4) The present invention uses vacuum molding to composite the modified quartz fiber cloth with the silicone resin matrix, which is simple to operate and is conducive to the combination of the modified quartz fiber cloth and the silicone resin matrix, thereby obtaining a modified quartz fiber / silicone resin composite material with excellent mechanical properties and heat resistance.

[0024] The preparation method of the present invention is simple to operate, and the prepared modified quartz fiber / silicone resin composite material has excellent mechanical properties, temperature resistance and high-temperature mechanical properties, and can be used to prepare high-temperature resistant antenna covers. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a flow chart for preparing the modified quartz fiber / silicone resin composite material;

[0026] Figure 2 Schematic diagram of the chemical reaction principle of quartz fiber surface modification. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] ①Quartz fiber modification

[0030] A quartz fiber cloth with a thickness of 0.1 mm and a mass of 300 g was placed in 600 g of acetone, refluxed at 60° C. for 6 hours, then washed with acetone 3 times, vacuum dried at 50° C., and refluxed-washed-dried three times to obtain a clean quartz fiber with the impregnant removed; the clean quartz fiber with the impregnant removed was placed in 200 g of 1.0 mol / L dilute nitric acid, reacted at 80° C. for 6 hours, and after the reaction was completed, it was washed with tetrahydrofuran, and then vacuum dried at a vacuum degree of -0.06 MPa and a temperature of 30° C. The hydroxylated quartz fiber was dried in an oven for 8 hours to obtain a hydroxylated quartz fiber; the hydroxylated quartz fiber was further placed in 600 g of tetrahydrofuran, and 7 g of methylphenylsilane, 5 g of dimethylsilane, 3 g of phenylsilane and 0.05 g of chloroplatinic acid catalyst were added, and the reaction was carried out at 80°C for 4 hours, and the reaction was cooled to room temperature after the reaction was completed; 36 g of dilute hydrochloric acid with a concentration of 0.04 mol / L was slowly added dropwise to the reaction system at a dropping rate of 2 mL / min, and the reaction was carried out at 70°C for 10 hours, and the modified quartz fiber was washed with anhydrous ethanol and dried to obtain the modified quartz fiber;

[0031] ②Prepreg preparation

[0032] The modified quartz fiber cloth and 200 g of hydroxy silicone resin with a hydroxy content of 3%, a phenyl content of 45%, and a molar ratio of organic groups to silicon atoms of 1.15:1 were placed in an oven at 80°C and heated for 2.5 hours, and then the silicone resin was quickly and evenly coated on the modified quartz fiber cloth, and cooled to room temperature to obtain a prepreg;

[0033] ③ Composite material preparation

[0034] The prepreg prepared as above was cut, aligned and laid on a flat mold, placed in a vacuum hot press, the vacuum of the vacuum hot press was evacuated to below 0.1 MPa, heated to 120°C and kept warm for 1 hour, then pressurized to 10 MPa, keeping the pressure constant, kept warm at 150°C for 1 hour, 200°C for 2 hours, and 250°C for 4 hours, cooled to room temperature and demolded to obtain a modified quartz fiber / silicone resin composite material-Sample I.

[0035] Comparative Example 1

[0036] The difference between this comparative example and Example 1 is that the quartz fiber uses unmodified quartz fiber, the preparation of the prepreg and the preparation of the composite material are the same as in Example 1, and an unmodified quartz fiber / silicone resin composite material - Sample II is prepared.

[0037] The properties of the modified quartz fiber / silicone resin composite material sample I and the unmodified quartz fiber / silicone resin composite material sample II prepared by the methods described in Example 1 and Comparative Example 1 are shown in Table 1. Compared with sample II, the 500°C flexural strength of sample I is increased by 238.8%, and the 500°C interlaminar shear strength is increased by 167.3%.

[0038]

[0039] Example 2

[0040] ①Quartz fiber modification

[0041] A quartz fiber cloth with a thickness of 0.2 mm and a mass of 450 g was placed in 500 g of acetone, refluxed at 55° C. for 5 hours, then washed with acetone three times, vacuum dried at 45° C., and refluxed-washed-dried three times to obtain a clean quartz fiber with the impregnant removed; the clean quartz fiber with the impregnant removed was placed in 800 g of a 0.5 mol / L dilute nitric acid solution, reacted at 70° C. for 8 hours, and after the reaction was completed, it was washed with tetrahydrofuran, and then dried in a vacuum oven at a vacuum degree of -0.06 MPa and a temperature of 30° C. for 5 hours to obtain a hydroxylated quartz fiber; the hydroxylated quartz fiber was further placed in 1000 g of tetrahydrofuran, and 15 g of methylphenylsilane, 10 g of dimethylsilane, 5 g of phenylsilane and 0.072 g of Karstedt catalyst was reacted at 70°C for 7 hours, and then cooled to room temperature. 36 g of dilute hydrochloric acid with a concentration of 0.03 mol / L was slowly added to the reaction system at a dropping rate of 4 mL / min, and reacted at 60°C for 8 hours. The modified quartz fiber was washed with anhydrous ethanol and dried to obtain the modified quartz fiber.

[0042] ②Prepreg preparation

[0043] The modified quartz fiber cloth and 250 g of hydroxy silicone resin with a hydroxyl content of 4.5%, a phenyl content of 35%, and a molar ratio of organic groups to silicon atoms of 1.25:1 were placed in a 70°C oven and heated for 3 hours. The silicone resin was then quickly and evenly coated on the modified quartz fiber cloth and cooled to room temperature to obtain a prepreg.

[0044] ③ Composite material preparation

[0045] The prepreg prepared as above was cut, aligned and laid on a flat mold, placed in a vacuum hot press, the vacuum of the vacuum hot press was evacuated to below 0.1 MPa, heated to 120°C and kept warm for 1 hour, then pressurized to 15 MPa, keeping the pressure unchanged, kept warm at 150°C for 1 hour, 200°C for 2 hours, and 250°C for 4 hours, cooled to room temperature and demolded to obtain a modified quartz fiber / silicone resin composite material-Sample III.

[0046] Comparative Example 2

[0047] The difference between this comparative example and Example 2 is that the quartz fiber uses unmodified quartz fiber, the preparation of the prepreg and the preparation of the composite material are the same as in Example 2, and an unmodified quartz fiber / silicone resin composite material - Sample IV is prepared.

[0048] The properties of the modified quartz fiber / silicone resin composite material sample III and the unmodified quartz fiber / silicone resin composite material sample IV prepared by the methods described in Example 2 and Comparative Example 2 are shown in Table 2. Compared with sample IV, sample III has a 500°C flexural strength increased by 237.6%, and a 500°C interlaminar shear strength increased by 182.9%.

[0049] Table 2

[0050]

[0051] Example 3

[0052] ①Quartz fiber modification

[0053] A quartz fiber with a thickness of 0.15 mm and a mass of 400 g was placed in 700 g of acetone, refluxed at 50° C. for 8 hours, then washed with acetone three times, vacuum dried at 40° C., and refluxed-washed-dried three times to obtain a clean quartz fiber with the impregnant removed; the clean quartz fiber with the impregnant removed was placed in 600 g of a 2.0 mol / L dilute nitric acid solution, reacted at 90° C. for 4 hours, and after the reaction was completed, it was washed with tetrahydrofuran, and then dried in a vacuum oven at a vacuum degree of -0.08 MPa and a temperature of 30° C. for 6 hours to obtain a hydroxylated quartz fiber; the hydroxylated quartz fiber was further placed in 800 g of tetrahydrofuran, and 5 g of methylphenylsilane, 5 g of dimethylsilane, 12 g of phenylsilane and 0.025 g of Karstedt catalyst was reacted at 70°C for 6 hours, and then cooled to room temperature after the reaction was completed; 50 g of dilute hydrochloric acid with a concentration of 0.02 mol / L was slowly added to the reaction system at a dropping rate of 5 mL / min, and reacted at 50°C for 8 hours, and the modified quartz fiber was washed with anhydrous ethanol and dried to obtain.

[0054] ②Prepreg preparation

[0055] The modified quartz fiber cloth and a hydroxyl silicone resin having a hydroxyl content of 4%, a phenyl content of 40%, and a molar ratio of organic groups to silicon atoms of 1.20:1 were placed in a 75°C oven and heated for 3 hours, and then the silicone resin was quickly and evenly coated on the modified quartz fiber cloth and cooled to room temperature to obtain a prepreg.

[0056] ③ Composite material preparation

[0057] The prepreg prepared as above was cut, aligned and laid on a flat mold, placed in a vacuum hot press, the vacuum of the vacuum hot press was evacuated to below 0.1 MPa, heated to 120°C and kept warm for 1 hour, then pressurized to 20 MPa, keeping the pressure constant, kept warm at 150°C for 1 hour, 200°C for 2 hours, and 250°C for 4 hours, cooled to room temperature and demolded to obtain a modified quartz fiber / silicone resin composite material-Sample V.

[0058] Comparative Example 3

[0059] The difference between this comparative example and Example 3 is that the quartz fiber uses unmodified quartz fiber, the preparation of the prepreg and the preparation of the composite material are the same as in Example 3, and an unmodified quartz fiber / silicone resin composite material - Sample VI is prepared.

[0060] The properties of the modified quartz fiber / silicone resin composite material sample V and the unmodified quartz fiber / silicone resin composite material sample VI prepared by the methods described in Example 3 and Comparative Example 3 are shown in Table 3. Compared with sample VI, the 500°C flexural strength of sample V is increased by 247.3%, and the 500°C interlaminar shear strength is increased by 202.4%.

[0061] Table 3

[0062]

[0063] Example 4

[0064] A quartz fiber with a thickness of 0.28 mm and a mass of 350 g was placed in 650 g of acetone and refluxed at 55° C. for 10 hours, then washed with acetone three times, vacuum dried at 45° C., and refluxed-washed-dried three times to obtain a clean quartz fiber with the impregnant removed; the clean quartz fiber with the impregnant removed was placed in 500 g of a 1.5 mol / L dilute nitric acid solution, reacted at 75° C. for 8 hours, and after the reaction was completed, it was washed with tetrahydrofuran, and then dried in a vacuum oven at a vacuum degree of -0.07 MPa and a temperature of 30° C. for 4 hours to obtain a hydroxylated quartz fiber; the hydroxylated quartz fiber was further placed in 700 g of tetrahydrofuran, and 5 g of methylphenylsilane, 12 g of dimethylsilane, 15 g of phenylsilane, and 0.032 g of Karstedt catalyst and 0.032g chloroplatinic acid catalyst were reacted at 60°C for 6h, and then cooled to room temperature after the reaction was completed; 42g of dilute hydrochloric acid with a concentration of 0.05mol / L was slowly added to the reaction system at a drop rate of 3mL / min, and reacted at 80°C for 6h, and the modified quartz fiber was washed with anhydrous ethanol and dried to obtain the modified quartz fiber;

[0065] ②Prepreg preparation

[0066] The modified quartz fiber cloth and a hydroxyl silicone resin having a hydroxyl content of 3.5%, a phenyl content of 50%, and a molar ratio of organic groups to silicon atoms of 1.18:1 were placed in a 70°C oven and heated for 4 hours, and then the silicone resin was quickly and evenly coated on the modified quartz fiber cloth and cooled to room temperature to obtain a prepreg.

[0067] ③ Composite material preparation

[0068] The prepreg prepared as above was cut, aligned and laid on a flat mold, placed in a vacuum hot press, the vacuum of the vacuum hot press was evacuated to below 0.1 MPa, heated to 120°C and kept warm for 1 hour, then pressurized to 12 MPa, keeping the pressure constant, kept warm at 150°C for 1 hour, 200°C for 2 hours, and 250°C for 4 hours, cooled to room temperature and demolded to obtain a quartz fiber / silicone resin composite material-Sample VII.

[0069] Comparative Example 4

[0070] The difference between this comparative example and Example 4 is that the quartz fiber uses unmodified quartz fiber, the preparation of the prepreg and the preparation of the composite material are the same as Example 4, and an unmodified quartz fiber / silicone resin composite material - Sample VIII is prepared.

[0071] The properties of the modified quartz fiber / silicone resin composite material sample VII and the unmodified quartz fiber / silicone resin composite material sample VIII prepared by the methods described in Example 4 and Comparative Example 4 are shown in Table 4. Compared with sample VIII, the 500°C flexural strength of sample VII is increased by 235.6%, and the 500°C interlaminar shear strength is increased by 155.1%.

[0072] Table 4

[0073]

[0074] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing modified quartz fiber, characterized in that: The following steps are involved: Step 1, removing the impregnating agent on the surface of the quartz fiber, and then placing it in a dilute nitric acid solution for reaction, and after the reaction is completed, washing it with tetrahydrofuran and vacuum drying it to obtain a hydroxylated quartz fiber; Step 2: placing the hydroxylated quartz fiber in tetrahydrofuran, then adding hydrosilane and a catalyst thereto and heating for reaction, and cooling to room temperature after the reaction is completed; Step 3: slowly drop a dilute hydrochloric acid solution into the reaction system of step 2 and heat to react. After the reaction is completed, wash with anhydrous ethanol and dry to obtain modified quartz fiber.

2. The preparation method according to claim 1, characterized in that: In step 1, the method for removing the wetting agent on the surface of the quartz fiber is: placing the quartz fiber in acetone for reflux, then washing with acetone, vacuum drying, and repeatedly reflux-washing-drying to obtain the quartz fiber with the wetting agent removed.

3. The preparation method according to claim 1, characterized in that: The mass ratio of the quartz fiber to the acetone for reflux is 100:50-200, the reflux temperature is 45-60° C., and the reflux time is 8-12 hours.

4. The preparation method according to claim 1, characterized in that: In step 1, the mass ratio of quartz fiber to dilute nitric acid solution is 100:50-200, the concentration of dilute nitric acid solution is 0.5-2.0 mol / L, the reaction temperature is 60-90° C., and the reaction time is 6-12 hours.

5. The preparation method according to claim 1, characterized in that: In step 1, the vacuum degree of vacuum drying is -0.1 to -0.06 MPa, the temperature is 30 to 50° C., and the drying time is 4 to 8 hours.

6. The preparation method according to claim 1, characterized in that: In step 2, the mass ratio of the quartz fiber to tetrahydrofuran is 100:150-300; the mass ratio of the quartz fiber to the hydrogen-containing silane is 100:2-10; the mass ratio of the catalyst to the hydrogen-containing silane is 0.01-0.5:100, the reaction temperature is 60-80°C, and the reaction time is 2-8 hours.

7. The preparation method according to claim 1 or 6, characterized in that: The hydrogen-containing silane is a composition of methylphenylsilane, dimethylsilane and phenylsilane, and the mass ratio of the three is 5-20:5-15:3-20; the catalyst includes a combination of one or more of chloroplatinic acid and Karstedt catalyst.

8. The preparation method according to claim 1, characterized in that: In step 3, the concentration of the dilute hydrochloric acid solution is 0.02-0.05 mol / L, the mass ratio of the dilute hydrochloric acid solution to the quartz fiber is 5-15:100, the dropping rate is 2-5 mL / min, the reaction temperature is 50-80° C., and the reaction time is 4-12 hours.

9. An application of modified quartz fiber prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The following steps are involved: The hydroxy silicone resin is heated and melted and coated on a modified quartz fiber cloth to obtain a prepreg, the prepreg is formed by vacuum molding, and high-temperature curing is performed to obtain a high-strength modified quartz fiber / silicone resin composite material.

10. The use according to claim 9, characterized in that: The hydroxy silicone resin has a hydroxyl value content of 3-8%, a phenyl content of 25%-50%, a molar ratio of organic groups to silicon atoms of 1.1-1.25:1, and a resin softening point of 50-60°C.

Citation Information

Cited By

  • Quartz fiber with yttrium oxide coating and preparation method thereof

    CN119430689A