Multifunctional chitosan-based hydrogel as well as preparation method and application thereof

The multifunctional hydrogel formed by self-polymerization of chitosan and aldehyde polyphenols solves the antibacterial and antioxidant problems in traditional technology, and achieves low-cost and simple preparation of photothermal antibacterial and antioxidant effects, significantly improving the wound Healing performance, providing solutions for new wound dressings.

CN118909319APending Publication Date: 2024-11-08THE EYE HOSPITAL OF WENZHOU MEDICAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410874876.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively antibacterial and antioxidant when dealing with skin trauma, and the use of antibiotics leads to the production of drug-resistant bacteria. Traditional photothermal hydrogels are cumbersome in preparation and the source of materials is not easy, which cannot meet the needs of wound healing.

Method used

The multifunctional hydrogel is formed by self-polymerization of chitosan and its derivatives with aldehyde polyphenols. The photothermal heating is used to kill bacteria and remove reactive oxygen, providing self-healing, injectable, photothermal antibacterial and antioxidant functions.

Benefits of technology

It realizes a low-cost, simple preparation of multifunctional hydrogels, with excellent cell compatibility and in vivo biosafety, significantly improves antibacterial and pro-repair performance, and provides a solution for new wound dressings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909319A_ABST
    Figure CN118909319A_ABST
Patent Text Reader

Abstract

The invention relates to a multifunctional chitosan-based hydrogel and a preparation method and application thereof, in particular to a multifunctional wound repairing hydrogel with self-repairing, photo-thermal antibacterial and antioxidant functions, the hydrogel is prepared only by using chitosan and derivatives thereof and aldehyde polyphenol as materials, and the hydrogel is formed through Schiff base and polyphenol auto-polymerization. Benefited from dynamic bond crosslinking, the hydrogel has self-repairing / injectable properties and the like, bacteria can be killed by utilizing the photo-thermal conversion heating effect after polyphenol auto-polymerization, and aldehyde polyphenol has a plurality of phenolic hydroxyl groups, so that the anti-oxidation capability is achieved; the feasibility of the hydrogel as a novel wound dressing for bacterial infection wounds is evaluated through in-vitro experiments and animal experiments, and the hydrogel is proved to have good cytocompatibility and in-vivo biological safety at the levels of cells, blood and animal tissues. In a bacterial infected full-thickness skin injury model, the hydrogel also shows excellent antibacterial and repair promoting performance, and the hydrogel which integrates photo-thermal antibacterial and antioxidant functions and is low in cost and easy to prepare provides a new thought for treating infected wounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to a multifunctional chitosan-based hydrogel and a preparation method and application thereof. Background Art

[0002] The skin is the largest organ in the human body. It plays a protective role as a barrier and is also the first line of defense for the body. It is very vulnerable to damage. Skin trauma is often accompanied by bacterial wound infection. During the wound healing process, bacterial infection will lead to excessive production of reactive oxygen species (ROS) at the wound site, which seriously hinders the transition of wound healing to the subsequent proliferation and remodeling stage, resulting in slow wound healing or even no healing. Therefore, antibacterial and antioxidant are important conditions for wound healing. In addition, the frequent use of antibiotics has led to the emergence of drug-resistant bacteria, and new non-antibiotic multifunctional biomaterials are urgently needed. Hydrogels have attracted widespread attention due to their good biocompatibility, ability to provide a moist environment to promote wound repair, prevent further bacterial infection, and strong plasticity. Photothermal therapy (PTT) is a new antibacterial strategy that uses photothermal agents to convert light energy into heat energy. Compared with traditional antibiotic therapy, it has the advantages of broad-spectrum antibacterial activity, targeted selectivity, deep tissue / biofilm penetration, remote controllability, rapid effectiveness, and fewer side effects. However, photothermal water gels with the above conditions are usually cumbersome to prepare, with a long cycle and difficult material sources. Summary of the invention

[0003] In order to solve the shortcomings of the prior art, the present invention provides a multifunctional chitosan-based hydrogel and a preparation method and application thereof. The hydrogel is prepared by taking chitosan and its derivatives and aldehyde polyphenol as materials, and the hydrogel is formed by self-polymerization of Schiff base and polyphenol. The hydrogel has the properties of self-repairing / injectable, and the photothermal warming effect of the self-polymerization product of polyphenol is used to kill bacteria. The aldehyde polyphenol carries multiple phenolic hydroxyl groups, which have the ability to remove ROS. The feasibility of using the hydrogel as a new wound dressing for bacterial infection wounds is evaluated through in vitro experiments and animal experiments. The low-cost and easy-to-prepare hydrogel with integrated self-repairing, injectable, photothermal antibacterial, antioxidant and other functions provides a new idea for treating infected wounds.

[0004] The technical solution adopted by the present invention is: a multifunctional chitosan-based hydrogel, wherein the multifunctional chitosan-based hydrogel is formed by the self-polymerization of chitosan and its derivatives and aldehyde polyphenols through Schiff base bonds and polyphenols, and the molar ratio of the aldehyde groups on the aldehyde polyphenols to the amino groups on the chitosan and its derivatives is 0.5-3:10.

[0005] The molar ratio of the aldehyde groups on the aldehyde polyphenol to the amino groups on the chitosan and its derivatives is 2:10.

[0006] The chitosan and its derivatives include one or more of carboxymethyl chitosan, quaternized chitosan and hydroxyethyl chitosan.

[0007] The aldehyde polyphenols include one or more of 2,3,4-trihydroxybenzaldehyde, 2,4,5-trihydroxybenzaldehyde and 3,4,5-trihydroxybenzaldehyde.

[0008] The multifunctional chitosan-based hydrogel is a hydrogel formed by self-polymerization of carboxymethyl chitosan and 3,4,5-trihydroxybenzaldehyde through Schiff base bonds and polyphenols.

[0009] A method for preparing a multifunctional chitosan-based hydrogel comprises the following steps: weighing chitosan and its derivatives into a bottle, adding PBS solution to dissolve after magnetic stirring, weighing aldehyde polyphenols to add into the bottle, stirring to make it self-polymerize to form a hydrogel.

[0010] Application of a multifunctional chitosan-based hydrogel in preparing a new wound dressing for bacterially infected wounds.

[0011] In the novel wound dressing for wounds infected with bacteria, the molar ratio of the aldehyde groups on the aldehyde polyphenols to the amino groups on the chitosan and its derivatives is 2:10.

[0012] The novel wound dressing for bacterial infection wound surface produces a photothermal conversion effect under 808 nm near-infrared laser irradiation.

[0013] The beneficial effects of the present invention are as follows: the present invention provides a multifunctional chitosan-based hydrogel and its preparation method and application, a multifunctional wound repair hydrogel with self-repairing, injectable, photothermal antibacterial and antioxidant functions, and only chitosan and its derivatives and aldehyde polyphenols are used as materials to prepare the hydrogel, and the hydrogel is formed by the self-polymerization of Schiff base and polyphenols. Photothermal heating is used to kill bacteria, and the aldehyde polyphenols carry multiple phenolic hydroxyl groups, which have the ability to remove ROS. The feasibility of using it as a new wound dressing for bacterial infection wounds is evaluated through in vitro experiments and animal experiments, and it is confirmed that the hydrogel has good cell compatibility and in vivo biosafety at the cell, blood and animal tissue levels. In the full-thickness skin injury model of bacterial infection, it also shows excellent antibacterial and repair-promoting properties. This low-cost and easy-to-prepare hydrogel with integrated photothermal antibacterial, antioxidant and other functions provides a new idea for the treatment of infected wounds. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 (A) Comparison of solution-gel transition of carboxymethyl chitosan mixed with 3,4,5-trihydroxybenzaldehyde (GA) and gallic acid, respectively, and (B) SEM micromorphology of CG hydrogel formed by carboxymethyl chitosan and GA.

[0015] Figure 2 (A) Self-healing property of CG hydrogel (B) Injectability.

[0016] Figure 3 (A) Mechanical strength of hydrogels with different GA concentrations (B) Oscillatory strain scanning (C) Viscosity change with shear rate (D) Strain step experiment.

[0017] Figure 4 is the swelling property of CG hydrogel.

[0018] Figure 5 (A) Temperature rise curves of CG hydrogels with different GA concentrations (B) Temperature rise curves of CG 0.2 hydrogels at different times (C) Photothermal temperature rise images of CG 0.2 hydrogels on animals (D) Photothermal stability test of CG 0.2 hydrogels (E) Temperature rise curves of CG 0.2 hydrogels on animals.

[0019] Figure 6 (A) ABTS free radical scavenging experiment (B) DPPH free radical scavenging experiment (C) PTIO free radical scavenging experiment (D) Hydroxyl free radical scavenging experiment.

[0020] Figure 7 Effects of different concentrations of CG hydrogel extracts on the survival rate of L929 cells after incubation for 24 h, 48 h and 72 h.

[0021] Figure 8 (A) Dilution plate of different treatment groups (B) Survival rate of Staphylococcus aureus bacteria.

[0022] Fig. 9 Healing outcomes of bacterially infected full-thickness skin wounds in rats at different times.

[0023] Fig.10 (A) Schematic diagram of wound area in each group (B) Statistical diagram of rat weight at different times in each group (C) Wound healing rate in each group (n=3).

[0024] Fig.11 Hemolysis rate of CG hydrogel. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1: Preparation of CG hydrogel 1) Weigh 0.2 g of carboxymethyl chitosan (CMCS) into a glass bottle, add 6 mL of PBS solution and stir to dissolve to obtain CMCS solution.

[0027] 2) Weigh 2.97 mg, 5.94 mg, and 8.91 mg of GA, respectively, and add them to the CMCS solution so that the ratio of the aldehyde group on GA to the amino group on CMCS is 1:10, 2:10, and 3:10. Stir to allow it to self-polymerize to form hydrogels, which are named CG 0.1, CG 0.2, and CG 0.3, respectively.

[0028] Example 2: Morphological characterization of CG hydrogel (SEM) Scanning electron microscopy (SEM) is an observation method between transmission electron microscopy and optical microscopy. It uses a focused narrow high-energy electron beam to scan samples, and stimulates various physical information through the interaction between the beam and the material. This information is collected, amplified, and re-imaged to achieve the purpose of characterizing the microscopic morphology of the material.

[0029] The experimental steps are as follows: 1) Place the prepared CG hydrogel in a 5 mL Eppendorf tube, place the Eppendorf tube in a -80°C refrigerator, and after it is completely frozen, quickly transfer it to a low-temperature freeze dryer for freeze drying for 72 hours for later use; 2) Cut the freeze-dried hydrogel into cross-sections and longitudinal sections respectively, and adhere them to the copper conductive glue, and adhere the copper conductive glue with the sample to the sample holder; 3) The samples were sprayed with gold to improve the conductivity and observed using SEM.

[0030] Example 3: Characterization of mechanical properties of CG hydrogel 1) Self-healing characterization Cut the CG hydrogel obliquely into two parts, then stick the two pieces of gel together. After waiting for 5 minutes, use tweezers to hold one part in the air to observe whether the cut surface is flat and whether the other part will fall off, and take photos to record the actual situation.

[0031] 2) Injectability characterization 1. Load the CG hydrogel into a 10 mL syringe, push the syringe to inject the hydrogel onto a white cardboard, and write on it to evaluate the injectability of the CG hydrogel and take photos to record the actual situation.

[0032] 2. In a 10 mL glass bottle filled with water, use the syringe containing the hydrogel mentioned above to push the syringe to inject the hydrogel underwater and take photos to record the actual situation.

[0033] Example 4: Rheological characterization of CG hydrogel The mechanical properties, self-healing properties, and injectability of CG hydrogels were determined by rotational rheometer, with 25 mm parallel aluminum plates at 25 °C.

[0034] 1) Frequency sweep experiment: In order to compare the mechanical properties, the strain was set constant at 1%, and the sweep frequency was 0.1-100 rad / s. The storage modulus (G') and loss modulus (G'') of the above CG 0.1, CG 0.2 and CG 0.3 were tested.

[0035] CG 0.2 was selected to further investigate their self-repairing and injectable capabilities.

[0036] 2) Oscillatory strain amplitude sweep: ranging from 0.1% to 1000% with a constant frequency of 1 Hz to determine the critical strain required for gel failure.

[0037] 3) Frequency sweep: 0.1−100 s -1 The viscosity change of the hydrogel was detected at a frequency of , so as to evaluate its shear thinning property, i.e., injectability.

[0038] 4) Strain step experiment: First, the critical strain required for the gel network to collapse was determined by oscillating strain amplitude scanning. Then, at a constant frequency, alternating strains (1% and 150%, with an interval of 60 s) were applied to the sample, and the storage modulus (G') and loss modulus (G'') of the gel were recorded over time to evaluate the self-healing behavior of the hydrogel.

[0039] Example 5: Swelling of CG hydrogel Swelling rate: Weigh the 5mL Ep tube in advance and record the weight as W Ep , put 1mL of hydrogel into the tube and freeze-dry it. Weigh the weight of the freeze-dried hydrogel with Ep tube as W Eg After a predetermined time, the PBS was removed and discarded, and the hydrogel was weighed and recorded as W. t Three samples were measured in each group, and the results were taken as the average value ± standard deviation. The swelling rate (SR) of the hydrogel was calculated by the following formula: Swelling Ratio (%) = (W t -(W Eg -W Ep )) / W d ×100% Example 6: Photothermal properties of CG hydrogel In order to verify whether CG gel has photothermal properties, the photothermal properties of the prepared CG hydrogel were evaluated using an 808 nm near-infrared laser. All samples were placed in a 1.5 mL Eppendorf tube and irradiated with an 808 nm laser at gradient powers (1.0, 1.5, and 2.0 W / cm 2 ) for 10 min. During the entire irradiation process, the temperature change of the sample was monitored by an infrared thermal imager (E60, FLIR, USA), with a picture taken every 30 s. In addition, the stability of the sample during three consecutive laser heating and cooling cycles, as well as the photothermal curves of the CG hydrogel at different time points after synthesis, were evaluated to describe the change of the photothermal effect with cross-linking time.

[0040] Example 7: Test of total antioxidant capacity of CG hydrogel In this experiment, different methods were used to evaluate the antioxidant capacity of CG hydrogel.

[0041] (1) Total antioxidant capacity test kit (ABTS method) ABTS is a colorimetric agent that will be oxidized to blue ABTS under the action of a suitable oxidant (such as potassium persulfate). ·+ , blue ABTS ·+ It is easily reduced to colorless by antioxidants, so the ABTS after the reaction is measured at 734 nm. ·+ The absorbance can be used to determine the total antioxidant capacity of the sample. The specific steps for detecting the total antioxidant capacity of CG hydrogel are as follows: 1) Dilute and mix the ABTS solution and oxidant provided in the kit according to the concentration in the instructions; 2) Add 1 mL of CG 0.1 hydrogel, CG 0.2 hydrogel, CG 0.3 hydrogel; 3) Transfer the mixed ABTS working solution into 5 mL transparent glass bottles at a rate of 3 mL per bottle, and quickly take photos and record; 4) After 0.5 h, take photos again and transfer some of the solutions to a 96-well plate. Use an ELISA reader to measure the absorbance of each solution at 734 nm and calculate the ABTS. ·+ Clearance rate; (2) DPPH · Free Radical Scavenging DPPH · It is a nitrogen-centered color-developing free radical with a characteristic absorption peak at 517nm. The addition of antioxidants will make DPPH · The absorbance decreased and the purple-red color disappeared. The clearance rate was calculated by measuring the absorbance of the corresponding absorption peak.· The specific steps of free radical are as follows: 1) Weigh 1.76 mg of DPPH powder and dissolve it in 23 mL of anhydrous ethanol to make a 0.2 mM DPPH solution. · Working fluid.

[0042] 2) Add 0.5 mL of CG 0.1 hydrogel, CG 0.2 hydrogel, and CG 0.3 hydrogel in order according to the group into a 5 mL transparent glass bottle; 3) Mix the DPPH · Transfer 1 mL of the working solution into the above-mentioned 5 mL transparent glass bottles and quickly take photos and record; 4) After 0.5 h, take photos again and transfer some of the solutions to a 96-well plate. Use an ELISA reader to measure the absorbance of each solution at 517 nm and calculate the DPPH. · Clearance rate; (3) PTIO · Free Radical Scavenging PTIO · It is an oxygen-centered chromogenic free radical. When dissolved in water (PBS buffer), the characteristic absorption peak is at 557 nm. When dissolved in organic solutions such as methanol and DMSO, the characteristic absorption peak is at 585 nm. · After dissolution, it is a purple solution. When antioxidants remove PTIO · When the solution is added, the color of the solution becomes lighter, and the clearance rate is calculated by measuring the absorbance of the corresponding absorption peak. · specific Here are the steps: 1) Weigh 2.92 mg of PTIO powder and dissolve it in 25 mL of pure water to prepare a 0.5 mM PTIO working solution.

[0043] 2) Add 0.5 mL of CG 0.1 hydrogel, CG 0.2 hydrogel, and CG 0.3 hydrogel in order according to the group into a 5 mL transparent glass bottle; 3) Mix the PTIO · Transfer 2.5 mL of the working solution into the above-mentioned 5 mL transparent glass bottles and quickly take photos and record; 4) After 1 hour, take photos again and transfer some of the solutions to a 96-well plate. Use an ELISA reader to measure the absorbance of each solution at 557 nm and calculate PTIO. · Clearance rate; (4) Hydroxyl radical scavenging method The Fenton reaction is used to generate hydroxyl radicals, which then react with salicylic acid to generate 2,3-dihydroxybenzoic acid with a special absorption peak at 510 nm. If a substance that can scavenge hydroxyl radicals is added, the generated hydroxyl radicals will be reduced, thereby reducing the amount of colored compounds generated and reducing the absorption at 510 nm. The scavenging rate is calculated by measuring the absorbance of the corresponding absorption peak. The specific steps for detecting the scavenging of hydroxyl radicals by CG hydrogel are as follows: 1) Weigh and dissolve FeSO4·7H2O in pure water to 2.50 mg / mL to prepare a 9 mM FeSO4 aqueous solution.

[0044] 2) Weigh and dissolve salicylic acid in anhydrous ethanol to 1.24 mg / mL to prepare a 9 mM salicylic acid ethanol solution.

[0045] 3) Dilute 1 M H2O2 to 4.4 mM H2O2 solution in a gradient manner.

[0046] 4) Mix equal volumes of the above-mentioned 9 mM FeSO4 aqueous solution, 9 mM salicylic acid ethanol solution and 4.4 mM H2O2 solution as a hydroxyl radical working solution for later use.

[0047] 5) Add 0.5 mL of CG 0.1 hydrogel, CG 0.2 hydrogel, and CG 0.3 hydrogel in order according to the groups into a 5 mL transparent glass bottle; 6) Transfer the mixed hydroxyl radical working solution into the above-mentioned 5 mL transparent glass bottles at a rate of 3 mL per bottle, and quickly take photos and record; 7) After 1 hour, take photos again and transfer some of the solutions to a 96-well plate. Use an ELISA reader to measure the absorbance of each group of solutions at 510 nm and calculate the hydroxyl radical scavenging rate.

[0048] Example 8: L929 cell viability assay (CCK-8) CCK-8 is a kit for detecting cell proliferation-toxicity. CCK-8 solution can enter cells and can be oxidized and reduced by dehydrogenases in living cells to generate highly water-soluble orange-yellow formazan dye. The amount of this dye generated is proportional to the number of living cells in culture and the incubation time. This experiment used the CCK-8 kit to evaluate the cell biological toxicity of different concentrations of CG extract on L929 cells, and 5 replicate wells were set for each group. The specific steps are as follows: 1) This experiment was divided into experimental group, control group and Blank group. Except for the Blank group, L929 cells were plated in 96-well plates according to the cell seeding method, with a cell number of 8×10 3Each well was plated with a volume of 100 μL and cultured in a constant temperature cell culture incubator at 37°C and 5% CO2 saturated humidity for 24 h until the cells were completely attached to the wall; 2) The materials required for gelation were sterilized by ultraviolet for 30 min, sterilized PBS was added to them to make them gel, and serum-containing cell culture medium was used to prepare CG 0.1, CG 0.2, and CG 0.3 hydrogel extracts (the volume ratio of gel to extract was 1:40) 3) Use a spray gun to remove the cell culture medium in the 96-well plate, add 100 μL of gel extract of different concentrations to the plate according to the experimental design, and place it in a constant temperature incubator at 37°C and 5% CO2 saturated humidity for 24 h, 48 h, and 72 h respectively; 4) After the set time of incubation, remove the culture medium in each well with a pipette, wash each well three times with D-Hank's, add 100 μL of cell culture medium containing 10% CCK-8 solution to each well (including Blank group) under light-proof conditions, and incubate at 37°C for 1-2 h; 5) Use an ELISA reader to measure the absorbance (OD) of the 96-well plate at 450 nm; 6) Calculate the cell survival rate using the formula: Cell viability % = (OD 实验组 -OD blank组 ) / (OD 对照组 -OD blank组 )×100% Example 9: Plate colony counting method The plate colony counting method is one of the most effective methods for counting the number of microbial colonies on items. The plate counting method can be used to evaluate the in vitro antibacterial activity of hydrogels. This experiment was divided into Control group, Control+NIR group, CG 0.1 group, CG 0.1+NIR group, CG 0.2 group, CG 0.2+NIR group, CG 0.3 group, and CG 0.3+NIR group, and the experiment was repeated three times. The specific steps are as follows: 1) Sterilize the materials required for gelation under UV for 30 min. After gelation, place them in a 24-well plate in a clean bench. The volume of the hydrogel is 0.8 mL. 2) Dilute the cultured bacterial suspension to 1×10 7 CFU / mL and reserve; 3) In a 24-well plate, add 1 mL of the above bacterial solution to the Control group, 1 mL of liquid culture medium to the Blank group, and 200 μL of the above bacterial solution to the experimental group; 4) The experimental group requiring NIR laser irradiation was 1.5 W / cm 2The cells were treated at a power of 10 min, and then 50 μL of bacterial solution was taken from each well plate and added to a shaking tube containing 5 mL of liquid culture medium, and cultured overnight in a tabletop constant temperature biological shaker (37°C, 100 r / min); 5) After the culture is completed, the bacterial suspension in the shaking tube is diluted with PBS in a gradient manner of 10 4 times, draw 50 μL and drop it onto the prepared solid culture medium, and spread it evenly on the solid culture medium with a bacterial spreader stick; 6) Finally, place the culture dish in a constant temperature incubator at 37°C and culture for 24 hours; 7) After cultivation, count the colonies and calculate the number of bacteria in the sample based on the dilution factor and the sample inoculation volume. Take a photo of the final cultivation result and count it based on the dilution factor and sample inoculation volume.

[0049] Example 10: Rat bacterial infection full-thickness skin injury model 1) Dilute the cultured Staphylococcus aureus bacterial suspension with saline to 1×10 6 CFU / mL and reserve; 2) Anesthetize the rats with isoflurane. After successful anesthesia, gently shave the hair on the back of the mice with an animal shaver (to avoid damaging the skin) and disinfect them. 3) Use a sterile circular skin punch with a diameter of 8 mm to make a full-thickness circular wound on the back of the rat; 4) Use a pipette to draw 10 μL of Staphylococcus aureus liquid and evenly distribute it on each wound surface to establish a bacterial infection wound model; 5) After 24 hours, white pus was observed on the wound surface of the rats, indicating that the model was successfully established.

[0050] Example 11: Evaluation of the therapeutic effect of CG hydrogel 1) SD rats were randomly divided into 4 groups. The control group was treated with 0.8 mL normal saline, the commercial dressing group was treated with 3M transparent film dressing, the CG 0.2 group was treated with 0.8 mL CG 0.2 hydrogel, and the CG 0.2+NIR group was treated with CG 0.2 hydrogel under NIR (1.5 W / cm 2 , 10 min) treatment; 2) Evaluation of wound surface healing: The wounds of rats were recorded and statistically analyzed on the 1st, 4th, 7th, 10th, and 14th days respectively; the wounds of each group were photographed and recorded with a camera. The area of ​​each wound was measured and statistically analyzed using Image J software, and the wound surface healing was evaluated. The ratio of the exposed wound area visible to the naked eye was used to express the wound healing situation. Wound healing rate (%) = (initial open wound area on the modeling day - open wound area on the photo-taking day) / initial open wound area on the modeling day × 100%; 3) Evaluation of rat body weight changes: The body weight of rats was recorded using an electronic scale on days 1, 4, 7, 10, and 14.

[0051] Example 12: Blood compatibility evaluation Good blood compatibility is a prerequisite for the application of biomaterials in wounds. Therefore, it is necessary to identify whether the blood compatibility of CG hydrogel is good. We use hemolysis test to verify whether it can be applied in wounds. The specific steps are as follows: 1) Grouping: The experiment was divided into PBS group (negative control), 0.1% Triton X-100 group (positive control), CG 0.1 group, CG 0.2 group, and CG 0.3 group.

[0052] 2) Sample collection: Take fresh whole blood from rats. Centrifuge for 5 minutes (at a speed of 3000 rpm), obtain the red blood cells in the lower layer, and rinse with PBS several times until the supernatant is colorless. Remove the supernatant and extract the pure red blood cells (RBC) precipitated at the bottom of the centrifuge tube for later use; 3) Dilution: Dilute the obtained red blood cells with PBS to a concentration of 5% (v / v).

[0053] 4) Centrifugation: For the negative control group, 0.3 mL of diluted red blood cell suspension was mixed with 1 mL of PBS, for the positive control group, 0.3 mL of diluted red blood cell suspension was mixed with 1 mL of 0.1% Triton X-100, and for the experimental group, 0.3 mL of diluted red blood cell suspension was mixed with 0.1 mL of gel + 0.9 mL of PBS. The above samples were shaken at 100 rpm for 1 h at 37°C, and then the mixture was centrifuged together for 5 min (speed was 8000 rpm); 5) Measurement: Use a pipette to transfer 100 μL of supernatant to a 96-well plate, and use a microplate reader to measure and record the absorbance value (Ab) of the supernatant at 540 nm. Use 0.1% Triton X-100 as a positive control sample (At), and PBS as a negative control sample (Ap). Calculate the hemolysis rate of the hydrogel according to the following formula: Hemolysis rate of hydrogel (%) = (Ab-Ap) / (At-Ap) × 100% Experimental results analysis (1) Solution-gel transition and SEM morphology characterization of CG hydrogel The present invention prepares CG hydrogel with photothermal and antioxidant properties by simply mixing CMCS with GA. Figure 1 As shown in A, GA (Gallic aldehyde, GA-COH) and gallic acid (Gallic acid, GA-COOH) with aldehyde groups replaced by carboxyl groups were used for gelation comparison. It can be seen that at 4 h, the CMCS solution with GA added formed a hydrogel, while the CMCS solution with gallic acid added did not form a hydrogel until 24 h. At the same time, it was observed that both mixed solutions changed color, which should be due to the self-polymerization reaction of polyphenols. This shows that CMCS forms Schiff base bonds with the aldehyde groups on GA and cross-links through self-polymerization to form a hydrogel. Figure 1 As shown in B, after freeze-drying, the hydrogel presents a three-dimensional porous structure, which is conducive to the absorption of wound exudate.

[0054] (2) Characterization of mechanical properties of CG hydrogel Hydrogels formed by dynamic covalent bonds often have unique properties, such as self-healing properties. In addition, hydrogels can be injected through a syringe. Dynamic Schiff base bonds give hydrogels self-healing properties. In order to intuitively demonstrate these significant features, macroscopic observations were performed. A whole piece of CG hydrogel was cut diagonally and then placed close together and left to stand for 5 minutes. It was found that it had healed and could be lifted up with tweezers ( Figure 2 A). Then the CG hydrogel was placed in a syringe, injected into water, and written on cardboard, etc., showing the injectable properties of the hydrogel ( Figure 2 B).

[0055] (3) Rheological analysis of CG hydrogel The mechanical properties of the hydrogels were evaluated by rheological tests. First, a frequency sweep was performed to compare the mechanical strength of the hydrogels with different GA concentrations. Figure 3 As shown in A, the storage modulus (G′) values ​​of CG 0.1, CG 0.2, and CG 0.3 (ω=1 Hz, γ=1%) are approximately 210, 800, and 930 Pa, respectively. We can see that the modulus of the hydrogel increases with the increase of GA concentration, but the improvement of mechanical strength becomes weak after the GA concentration increases to 0.2-0.3. Subsequently, an oscillatory strain sweep from 0.1% to 1000% was performed at a fixed frequency of 1 Hz ( Figure 3B). G′ and G″ remain stable at low strain (within the linear viscoelastic platform). When the strain value gradually increases, G′ begins to decrease and is exceeded by G″, indicating that the hydrogel network is destroyed. The critical strain value for the rupture of CG 0.2 gel (when G′=G″) is about 117%. At the same time, the shear thinning behavior of the hydrogel was also studied by shear rate-viscosity scanning. Figure 3 As shown in Figure C, as the shear rate increases, the viscosity of the CG 0.2 hydrogel decreases, indicating that they have shear thinning properties, which makes them injectable. Finally, the self-healing ability of the designed hydrogel was verified by strain step alternation experiments ( Figure 3 D). It can be observed that after the gel network is destroyed (γ=300%), the hydrogel network can be quickly rebuilt (γ=1%) and is repeatable in at least 3 cycles of testing, indicating that CG hydrogel has excellent rapid and repeatable self-healing properties.

[0056] (4) Swelling properties of CG hydrogel The three-dimensional porous structure of the hydrogel enables it to have good water retention and the ability to absorb excess tissue exudate, which is beneficial to wound healing. Therefore, the swelling rate of hydrogels with different GA concentrations was studied, and the results are as follows Figure 4 As shown in the figure, it can be seen that CG hydrogels of all concentrations have excellent swelling properties and can basically reach swelling equilibrium after 3 hours, indicating that CG hydrogels have good water holding capacity and water absorption properties.

[0057] (5) Photothermal properties of CG hydrogel In order to evaluate the photothermal properties of CG hydrogels, Figure 5 As shown in A, under different GA concentration conditions, the 808 nm near-infrared laser (1.5 W / cm 2 The photothermal properties of CG hydrogels of different concentrations were tested by measuring the temperature change of the hydrogel under irradiation (10 min, 25 °C). The results showed a concentration-dependent photothermal conversion property. The temperature change of the CG0.2 group was nearly 35 °C, and some key enzymes related to bacterial life activities could be inactivated here, which could also cause bacterial cell membrane rupture and death. In order to explore the photothermal properties of CG hydrogels during gel formation, the photothermal properties of CG 0.2 hydrogels were tested at different times ( Figure 5 B). The data show that the photothermal conversion performance of the gel increases with time, which indicates that the polyphenols are continuously self-polymerizing during the process. After about 4 hours, its photothermal performance tends to be stable, indicating that the reaction is basically complete at this time, which also corresponds to the gelation time. In addition, the CG 0.2 hydrogel can still maintain good photothermal stability after 3 heating-cooling cycles, and the highest heating temperature has almost no significant decrease ( Figure 5D). Next, we used the same lighting conditions and the same CG 0.2 hydrogel to conduct a temperature increase test on the animal's back. Figure 5 As shown in C, the gel can be heated to about 55°C, with a change of about 17°C. The temperature change curve is as follows Figure 5 The above results indicate that the prepared CG hydrogel has excellent photothermal properties and has great potential as a photothermal antibacterial system for the treatment of bacterial infections.

[0058] (6) Antioxidant properties of CG hydrogel Excessive free radicals can induce damage to biological systems, and the ability of biomaterials to scavenge free radicals is of great significance for protecting cells, blood components and biomolecules from oxidative damage. Incorporating antioxidants into wound dressings can effectively reduce oxidative stress, accelerate enzyme repair, and improve metabolism by eliminating excess ROS, thereby promoting wound healing. In CG hydrogels, GA shows potential as an antioxidant, attributed to its rich phenolic hydroxyl groups. On this basis, the in vitro antioxidant activity of CG hydrogels was evaluated using the ABTS method, DPPH method, PTIO method, and hydroxyl radical scavenging experiments. We tested the antioxidant capacity of CG 0.1, CG 0.2, and CG 0.3, and the results showed that CG hydrogels were concentration-dependent in scavenging various free radical activities. For ABTS and DPPH, more than half of them can be removed in 30 min ( Figure 6 A, Figure 6 B) For PTIO and hydroxyl radicals, 60 min also has a good scavenging effect ( Figure 6 C, Figure 6 D). The above results indicate that CG hydrogel exhibits strong antioxidant activity.

[0059] (7) CCK-8 Good biocompatibility is a necessary prerequisite for the application of hydrogel dressings in future biomedicine. L929 cells were used to evaluate the cell biocompatibility of CG hydrogel. First, the CCK-8 kit was used to evaluate the effect of CG hydrogels with different GA concentrations on the survival rate of L929. Figure 7 As shown, compared with the control group, the cell viability was higher than 85% after 1, 2, and 3 days of co-culture with the gel extract, indicating that CG did not cause obvious toxicity to L929.

[0060] (8) Plate colony count The excellent photothermal activity of CG hydrogel provides a solid foundation for its antibacterial properties. In this study, we selected Staphylococcus aureus ( S. aureus) were used as representatives to study the photothermal antibacterial ability of CG hydrogels. First, we conducted a dilution plate experiment to evaluate the antibacterial effect. It is worth noting that compared with the other groups, the CG 0.2+NIR group and CG 0.3+NIR showed better antibacterial activity, with almost no single colonies appearing ( Figure 8 A). We also calculated the bacterial survival rate by counting the colonies on the plate. The experimental results showed that the inhibition rate of CG 0.2+NIR group on Staphylococcus aureus was close to 100% ( Figure 8 B).

[0061] (9) Results of bacterial infection wound healing experiment in rats The skin is a barrier against bacteria, and re-epithelialization is an important process in wound healing. The effect of CG hydrogel dressing on promoting the healing of infected wounds was studied in a full-thickness skin defect infection model of SD rats (e.g. Fig. 9 As shown). White pus appeared in the wound, proving that the model was successful. As time went on, after treatment in the Control group (normal saline group), 3M group (commercial dressing group), CG 0.2 group, and CG 0.2+NIR group, the wound area infected with bacteria gradually decreased, but there were significant differences in the specific degree of wound healing among the groups. The wound healing speed of the CG 0.2+NIR group was the fastest during the entire treatment process, and it was almost completely healed on the 14th day, indicating that the CG 0.2+NIR group had a stronger promoting effect on wound healing.

[0062] (10) Healing results of bacterially infected full-thickness skin wounds in rats at different times Fig.10 A shows the wound repair status of each group at 1, 4, 7, 10, and 14 days. It can be clearly seen that the wound closure in the CG 0.2+NIR group was the most obvious. Fig.10 As shown in C, on the 7th day, the wound healing rates of the CG 0.2+NIR group were approximately 58% and 63% higher than those of the Control group and the 3M group, respectively (p<0.01). Similar results were obtained on the 10th day. On the 14th day, the wound area of ​​each group was significantly reduced, and the wound healing rate of the CG 0.2 group was higher than that of the Control group and the 3M group, indicating that CG hydrogel also has a certain promoting effect on wound healing. The wound healing rate of the CG 0.2+NIR group was approximately 97.8%, indicating that the CG 0.2+NIR group has a more significant promoting effect on wound healing. The rats in each group were weighed and counted on days 1, 4, 7, 10, and 14 ( Fig.10 B) During the experiment, the body weight increased to a certain extent, indicating that the hydrogel and near-infrared photothermal treatment did not cause any harm to their life and health and had good safety.

[0063] (11) Blood safety evaluation According to the evaluation standard of the International Organization for Standardization (ISO) 10993-4, when the hemolysis rate is less than 5%, the hydrogel can be used for clinical use. Fig.11 As shown in the figure, after CG hydrogel was incubated with blood for 1 hour, there was no visible hemolysis. The hemolysis rates of CG0.1, CG 0.2, and CG 0.3 groups were approximately 0.69%, 1.25%, and 2.55%, respectively, all lower than the international standard of 5%. The results show that CG hydrogel has a low hemolysis rate and meets the application requirements for wound dressing.

[0064] Summary of experimental results Multifunctional CG hydrogel with a three-dimensional porous microstructure can be prepared by simply blending carboxymethyl chitosan CMCS solution and aldehyde polyphenol GA. The good self-healing and injectable properties of CG hydrogel were confirmed by rheological tests and macroscopic observations. The scavenging experiments of ABTS, DPPH, PTIO and hydroxyl radicals verified that CG hydrogel had good antioxidant capacity. The photothermal conversion performance of the hydrogel gradually improved during its gelation process and tended to be stable at about 4 h, and it showed good photothermal conversion performance that was dependent on GA concentration and could be repeated many times. The coating plate experiment confirmed that CG hydrogel had excellent antibacterial properties under 808 nm near-infrared light irradiation. The hydrogel was confirmed to have good biosafety at the cell, blood and animal tissue levels. In the full-thickness skin injury model of bacterial infection, the CG 0.2 + NIR group also showed excellent performance in promoting wound repair.

[0065] Summarize The present invention successfully prepared a CG multifunctional hydrogel based on all-natural products through a simple method, which has the following capabilities: (1) excellent self-repair / injectability, mainly due to dynamic Schiff base cross-linking; (2) good antioxidant capacity, which can quickly remove ABTS ·+ DPPH + PTIO + , hydroxyl radicals and other free radicals; (3) Excellent near-infrared photothermal conversion and antibacterial ability, with an in vitro killing rate of Staphylococcus aureus close to 100%. In animal experiments, it was found that CG hydrogel had better antibacterial and repair effects than commercial dressings under near-infrared light, thereby achieving more efficient treatment effects. At the same time, CG hydrogel showed good biocompatibility at both the cellular and animal levels. Therefore, CG hydrogel is a safe and efficient new type of wound dressing. This study is expected to provide new ideas for the development of new dressings for the treatment of bacterial infection wounds.

[0066] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

[0067] Technical personnel should note: Although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention. Any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. A multifunctional chitosan-based hydrogel, characterized in that: The multifunctional chitosan-based hydrogel is formed by the self-polymerization of chitosan and its derivatives and aldehyde polyphenols through Schiff base bonds and polyphenols, and the molar ratio of the aldehyde groups on the aldehyde polyphenols to the amino groups on the chitosan and its derivatives is 0.5-3:

10.

2. The multifunctional chitosan-based hydrogel according to claim 1, characterized in that: The molar ratio of the aldehyde groups on the aldehyde polyphenol to the amino groups on the chitosan and its derivatives is 2:

10.

3. The multifunctional chitosan-based hydrogel according to claim 1, characterized in that: The chitosan and its derivatives include one or more of carboxymethyl chitosan, quaternized chitosan and hydroxyethyl chitosan.

4. The multifunctional chitosan-based hydrogel according to claim 1, characterized in that: The aldehyde polyphenols include one or more of 2,3,4-trihydroxybenzaldehyde, 2,4,5-trihydroxybenzaldehyde and 3,4,5-trihydroxybenzaldehyde.

5. The multifunctional chitosan-based hydrogel according to claim 4, characterized in that: The dual-multifunctional chitosan-based hydrogel is a hydrogel formed by self-polymerization of carboxymethyl chitosan and 3,4,5-trihydroxybenzaldehyde through Schiff base bonds and polyphenols.

6. A method for preparing the multifunctional chitosan-based hydrogel according to claim 1, characterized in that: The method comprises the following steps: weighing chitosan and its derivatives into a bottle, adding PBS solution to dissolve after magnetic stirring, weighing aldehyde polyphenols to add into the bottle, stirring to make them self-polymerize and cross-link to form hydrogel.

7. Use of the multifunctional chitosan-based hydrogel according to claim 1 in preparing a novel wound dressing for bacterially infected wounds.

8. The use according to claim 7, characterized in that: In the novel wound dressing for wounds infected with bacteria, the molar ratio of the aldehyde groups on the aldehyde polyphenols to the amino groups on the chitosan and its derivatives is 2:

10.