Compound toughened needle-pricking-resistant WF modified natural rubber as well as preparation method and application of compound toughened needle-pricking-resistant WF modified natural rubber
By adding natural mulberry twig extract DNJ to natural rubber, a compounded, toughened, and needle-resistant WF-modified natural rubber was prepared. This solved the problem of toughness and needle resistance of natural rubber in harsh environments, improved the performance of rubber products, and simplified the production process.
Patent Information
- Application Number
- CN202411311281.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
AI Technical Summary
The poor toughness and needle resistance of natural rubber in harsh environments make rubber products prone to cracking in mines, mixed road surfaces, and cold environments, thus limiting their application.
Using natural mulberry twig extract DNJ (1-deoxynojirimycin) as a modifier, it is compounded with natural rubber latex. Through dilution, emulsification, stabilization and dispersion treatment, compounded toughened and needle-resistant WF modified natural rubber is prepared, avoiding the use of flocculants and simplifying the preparation process.
It improves the needle resistance, super toughness and tear resistance of rubber, reduces water pollution, lowers energy consumption, and enables industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber preparation, in particular to a compounded toughened and needle-resistant WF-modified natural rubber and a preparation method and application thereof. Background Art
[0002] In rubber products such as tires, although natural rubber has excellent properties such as elasticity, strength, wear resistance, and flex resistance, its toughness and needle resistance are extremely poor in mines, mixed roads, and harsh environments, especially in the cold winter in Northeast China, where it is more prone to cracking. This has caused many restrictions and instabilities in its actual application, especially under the influence of today's environment. The demand for high-performance rubber products in harsh environments has received more and more attention and research. Summary of the invention
[0003] The present invention aims at the shortcomings and deficiencies in the prior art. The present invention provides a compound toughened and needle-resistant WF modified natural rubber which can replace the raw rubber in the formula of rubber products such as tires, overcomes the problems of the original WF rubber being not resistant to needle puncture, having low toughness, and having flower chipping and falling pieces, and compounding DNJ (1-deoxynojirimycin), a natural mulberry branch extract, as a modified WF. After being applied to the tread, sidewall and other parts of the tire, the compound toughened and needle-resistant WF modified natural rubber is resistant to needle puncture, has super toughness, is tear-resistant and prevents flower chipping and falling pieces, and the preparation method and application thereof.
[0004] To achieve the above purpose, the present invention is implemented by the following technical scheme: the compound toughened needle-resistant WF modified natural rubber provided by the present invention comprises the following components by weight: natural rubber latex, diluent, emulsifier, dispersant, toughening agent; the natural rubber latex has a rubber latex dry content of 25%-42%, the diluent is an ammonia aqueous solution with a mass fraction of 0.50%-5.00%, and the diluent is added in an amount of 10%-80% of the dry content of the natural rubber latex;
[0005] The emulsifier is an emulsifier of one or more long-chain compounds in a straight chain or branched chain containing 15 to 25 carbon atoms; the amount of the emulsifier added is 0.02% to 1.50% of the dry content of the natural rubber latex;
[0006] The dispersant is one or more compounds containing 2-16 carbon atoms in a straight chain or branched chain; the amount of the dispersant added is 0.02%-0.90% of the dry content of the natural rubber latex;
[0007] The toughening agent is a modifier of a straight chain or branched compound containing 5 to 10 carbon atoms, and the toughening agent is a pure natural mulberry branch extract DNJ; the addition amount of the toughening agent is 2.00% to 10.00% of the dry content of the natural rubber latex.
[0008] Preferably, the toughening agent is specifically DNJ (1-deoxynojirimycin) C6H 13 NO4 white powder.
[0009] Preferably, the emulsifier is specifically long-chain octylphenol polyoxyethylene ether, dodecyltrimethylammonium chloride, polyglycerol fatty acid ester, fatty acid polyglycerol ester, any one or two thereof.
[0010] Preferably, the composition further comprises a stabilizer, wherein the stabilizer is any one of guaiacol, cresol, methylcresol and o-ethylphenol.
[0011] Preferably, the stabilizer is guaiacol extracted from pine tar oil.
[0012] Preferably, the dispersant is any one of erucamide, polyglycerol fatty acid ester, polyvinyl alcohol, vinyl alcohol copolymer, vinyl acetate-maleic anhydride copolymer, and polyacrylic acid.
[0013] Preferably, the natural rubber latex is fresh latex newly cut from rubber trees, or ammonia-added natural rubber latex.
[0014] The method for preparing the compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0015] (1) diluting the natural rubber latex with a diluent; diluting the natural rubber latex with the diluent to a concentration of 20%-40%, stirring evenly at a temperature of 20°C-60°C, at 30-60S / 50-100r / min, to obtain a natural latex dilution;
[0016] (2) in a weakly alkaline state, preparing an emulsifier / stabilizer of a certain concentration, dispersing the emulsifier in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 70° C. at a temperature of 30 to 60 seconds and 50 to 100 revolutions per minute to obtain an emulsified natural rubber latex;
[0017] Dispersing the stabilizer in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 60° C. at a temperature of 30 to 60 seconds and 50 to 100 revolutions per minute to obtain a stabilized natural rubber latex;
[0018] (3) mixing the toughening agent and the dispersant with the natural rubber latex obtained in step (2); stirring and compounding at a temperature of 20° C. to 60° C.;
[0019] Dispersing the dispersant in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 60° C. for 30 to 60 seconds and 50 to 100 revolutions per minute to obtain a dispersed natural rubber latex;
[0020] Dispersing the toughening agent in the natural rubber latex dilution obtained in step (1), stirring at high speed for 1 min-5 min / 500-1000 r / min at room temperature, to obtain a modified natural rubber latex;
[0021] (4) After the reaction is completed, demulsification and flocculation are carried out, and the composite micelles (flocs) after flocculation are creped, washed, hammer-milled and granulated to obtain the finished product after drying, thereby obtaining a needle-resistant and toughened modified natural rubber latex.
[0022] The invention discloses an application of a compound toughened and needle-resistant WF modified natural rubber, wherein the compound toughened and needle-resistant WF modified natural rubber is used in tire manufacturing.
[0023] The present invention provides a compound toughened and needle-resistant WF modified natural rubber and its preparation method and application. It has the following beneficial effects:
[0024] (1) The compound toughened needle-resistant WF modified natural rubber of the present invention and its preparation method and application, the performance of the modified WF modified natural rubber, in addition to maintaining the original physical properties, its biggest feature is that it has strong needle resistance, super toughness, tear resistance and prevention of chipping and falling pieces.
[0025] The invention adopts DNJ (1-deoxynojirimycin) extracted from natural mulberry branches as modified natural rubber, which is directly added into natural rubber latex to produce a preparation method and processing equipment of a compounded toughened and needle-resistant modified natural rubber latex.
[0026] (2) The compound toughened and needle-resistant WF modified natural rubber of the present invention uses pure natural mulberry branch extract DNJ (1-deoxynojirimycin) as a natural rubber latex modifier, and contains a variety of biologically active ingredients, polyhydroxy alkaloids, such as carbohydrates, fatty acids, cellulose and polysaccharides. Compared with traditional WF natural rubber, the present invention can achieve demulsification and flocculation of natural rubber latex without adding flocculants. Since no flocculants such as acid and salt are added, water washing is not required, thereby reducing water pollution; the preparation process is simple, the energy consumption is low, and it can be directly processed and produced on the basis of the original production line, and industrial production can be realized. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0028] Example 1
[0029] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0030] A1. Weigh 500 kg of natural rubber latex with a dry rubber content of 36% of freshly cut rubber, wherein the dry rubber content is 180 kg;
[0031] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 220 kg of pure water, and then weighed 1.1 kg of 36% concentration of ammonia water, at 25 ° C temperature 30-60S / 50-100r / min stirring, to obtain a 25% concentration of natural rubber latex dilution;
[0032] A3, weigh the emulsifier long chain octylphenol polyoxyethylene ether C 18 H 30 O3, 0.036 kg of colorless liquid, is dissolved in an equal proportion of 70°C hot water and stirred to mix evenly.
[0033] A4. Disperse the diluted emulsifier in the 25% natural rubber latex prepared in step A1, and stir evenly at 25°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0034] A5. Weigh 0.108 kg of the stabilizer guaiacol, dissolve it in an equal proportion of hot water at 29° C., stir and mix evenly, disperse the diluted stabilizer in the emulsified natural rubber emulsion obtained in step A4, stir evenly at 30° C. at 30-60 s / 50-100 r / min to obtain a stabilized natural rubber emulsion.
[0035] A6. Weigh 0.054 kg of polyglycerol fatty acid ester as a dispersant, dissolve it in an equal proportion of 90° C. hot water, stir and mix evenly, disperse the diluted dispersant in the stabilized natural rubber emulsion obtained in step A5, stir evenly at 30° C. at 30-60S / 50-100r / min to obtain a dispersed natural rubber emulsion.
[0036] A7. Weigh 3.85 kg of toughening agent DNJ (1-deoxynojirimycin), dissolve it in an equal proportion of 40° C. hot water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 30° C. at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0037] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0038] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0039] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0040] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0041] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0042] A13. After drying, the finished product is a needle-resistant and toughened modified natural rubber latex, which is subjected to full physical and chemical performance tests.
[0043] Example 2
[0044] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0045] A1. Weigh 500 kg of fresh natural rubber latex with a dry rubber content of 35%, wherein the dry rubber content is 175 kg;
[0046] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 200 kg of pure water, and then weighed 1.0 kg of 36% concentration of ammonia water, stirred at 40 ° C at 30-60S / 50-100r / min to obtain a 25% concentration of natural latex dilution;
[0047] A3, weigh the emulsifier dodecyl trimethyl ammonium chloride (C 15 H 34 Dissolve 0.0525 kg of ClN cationic emulsifier in 70°C hot water in equal proportion and stir to mix evenly.
[0048] A4. Disperse the diluted emulsifier in the 25% natural rubber latex prepared in step A1, and stir evenly at 40°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0049] A5. Weigh 0.105 kg of stabilizer methylcresol (C7H8O colorless crystals, slightly soluble in water), dissolve it in an equal proportion of 60°C hot water, stir and mix evenly, disperse the diluted stabilizer in the emulsified natural rubber emulsion obtained in step A4, stir evenly at 40°C at 30-60S / 50-100r / min to obtain a stabilized natural rubber emulsion.
[0050] A6, weigh 0.0525 kg of dispersant polyacrylic acid, dissolve it in 90°C hot water in equal proportion, and stir to mix evenly. Disperse the diluted dispersant in the stabilized natural rubber emulsion obtained in step A5, stir evenly at 40°C and 30-60S / 50-100r / min to obtain dispersed natural rubber emulsion.
[0051] A7. Weigh 4.025 kg of toughening agent DNJ (1-deoxynojirimycin), dissolve it in an equal proportion of 30° C. hot water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 30° C. at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0052] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0053] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0054] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0055] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0056] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0057] A13. After drying, the finished product is a needle-resistant and toughened modified natural rubber latex, which is subjected to full physical and chemical performance tests.
[0058] Example 3
[0059] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0060] A1. Weigh 600 kg of natural rubber latex with a dry rubber content of 30% of freshly cut rubber, wherein the dry rubber content is 180 kg of dry rubber;
[0061] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 120 kg of pure water, and then weighed 0.72 kg of 36% concentration of ammonia water, stirred at 50 ° C at 30-60S / 50-100r / min to obtain a 25% concentration of natural rubber latex dilution;
[0062] A3. Weigh 0.072 kg of emulsifier triglycerol monostearate, dissolve it in an equal proportion of 50°C hot water, and stir to mix evenly.
[0063] A4. Disperse the diluted emulsifier in the 25% natural rubber latex obtained in step A1, and stir evenly at 50°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0064] A5. Weigh the stabilizer o-ethylphenol (C8H 100.126 kg of O white crystalline powder, slightly soluble in water) is dissolved in an equal proportion of 70°C hot water, and stirred to mix evenly. The diluted stabilizer dispersant is dispersed in the emulsified natural rubber emulsion obtained in step A4, and stirred evenly at 50°C at 30-60S / 50-100r / min to obtain a stabilized natural rubber emulsion.
[0065] A6. Weigh 0.09 kg of dispersant vinyl alcohol copolymer (C4H8O), dissolve it in an equal proportion of 90°C hot water, stir and mix evenly, disperse the diluted dispersant in the stabilized natural rubber latex obtained in step A5, stir evenly at 50°C at 30-60S / 50-100r / min to obtain a dispersed natural rubber latex.
[0066] A7. Weigh 6.80 kg of toughening agent DNJ (1-deoxynojirimycin), dissolve it in an equal proportion of 30° C. hot water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 50° C. at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0067] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0068] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0069] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0070] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0071] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0072] A13. After drying, the finished product is a needle-resistant and toughened modified natural rubber latex, which is subjected to full physical and chemical performance tests.
[0073] Example 4
[0074] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0075] A1. Weigh 600 kg of freshly cut natural rubber latex with a dry rubber content of 28%, of which the dry rubber content is 168 kg;
[0076] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 72 kg of pure water, and then weighed 0.432 kg of 36% concentration of ammonia water, stirred at 25 ° C at 30-60S / 50-100r / min to obtain a 25% concentration of natural rubber latex dilution;
[0077] A3. Weigh 0.084 kg of emulsifier polyglycerol fatty acid ester, disperse it in an equal proportion of 80°C hot water, and stir to mix evenly.
[0078] A5. Weigh 0.1176 kg of the stabilizer guaiacol, dissolve it in an equal proportion of hot water at 29° C., stir and mix evenly, disperse the diluted stabilizer in the emulsified natural rubber emulsion obtained in step A4, stir evenly at 30° C. and 30-60S / 50-100r / min to obtain a stabilized natural rubber emulsion.
[0079] A4. Disperse the diluted emulsifier in the 25% natural rubber latex obtained in step A1, and stir evenly at 30°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0080] A6, weigh 0.084 kg of polyvinyl alcohol as dispersant, dissolve it in 95°C hot water in equal proportion, and stir to mix evenly. Disperse the diluted dispersant in the stabilized natural rubber latex obtained in step A5, and stir evenly at 30°C and 30-60S / 50-100r / min to obtain a dispersed natural rubber latex.
[0081] A7. Weigh 8.40 kg of toughening agent DNJ (1-deoxynojirimycin), dissolve it in an equal proportion of room temperature water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 30°C at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0082] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0083] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0084] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0085] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0086] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0087] A13. After drying, the finished product is a needle-resistant and toughened modified natural rubber latex, which is subjected to full physical and chemical performance tests.
[0088] Example 5
[0089] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0090] A1. Weigh 500 kg of natural rubber latex with a dry rubber content of 34% of freshly cut rubber, of which the dry rubber content is 170 kg;
[0091] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 180 kg of pure water, and then weighed 1.08 kg of 36% concentration of ammonia water, at 30 ° C temperature 30-60S / 50-100r / min stirring, to obtain a 25% concentration of natural rubber latex dilution;
[0092] A3. Weigh 0.085 kg of emulsifier dodecyltrimethylammonium chloride, disperse it in an equal proportion of 80°C hot water, and stir to mix evenly.
[0093] A4. Disperse the diluted emulsifier in the 25% natural rubber latex obtained in step A1, and stir evenly at 30°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0094] A5. Weigh 0.119 kg of the stabilizer guaiacol, dissolve it in an equal proportion of 29° C. hot water, and stir to mix evenly. Disperse the diluted stabilizer in the emulsified natural rubber emulsion obtained in step A4, and stir evenly at 30° C. at 30-60 s / 50-100 r / min to obtain a stabilized natural rubber emulsion.
[0095] A6. Weigh 0.084 kg of polyvinyl alcohol as a dispersant, dissolve it in an equal proportion of 95° C. hot water, stir and mix evenly, disperse the diluted dispersant in the stabilized natural rubber latex obtained in step A5, stir evenly at 30° C. at 30-60S / 50-100r / min to obtain a dispersed natural rubber latex.
[0096] A7. Weigh 8.40 kg of toughening agent DNJ (1-deoxynojirimycin), dissolve it in an equal proportion of room temperature water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 30°C at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0097] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0098] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0099] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0100] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0101] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0102] A13. After drying, the finished product is a needle-resistant and toughened modified natural rubber latex, which is subjected to full physical and chemical performance tests.
[0103] Control group 1
[0104] The method for preparing a compound toughened and needle-resistant WF-modified natural rubber comprises the following steps:
[0105] A1. Weigh 500 kg of natural rubber latex with a dry rubber content of 36% of freshly cut rubber, wherein the dry rubber content is 180 kg;
[0106] A2, 25% concentration of natural rubber latex, diluted with diluent, weighed 220 kg of pure water, and then weighed 1.1 kg of 36% concentration of ammonia water, at 25 ° C temperature 30-60S / 50-100r / min stirring, to obtain a 25% concentration of natural rubber latex dilution;
[0107] A3, weigh the emulsifier long chain octylphenol polyoxyethylene ether C 18 H 30 O3, 0.036 kg of colorless liquid, is dissolved in an equal proportion of 70°C hot water and stirred to mix evenly.
[0108] A4. Disperse the diluted emulsifier in the 25% natural rubber latex prepared in step A1, and stir evenly at 25°C at 30-60S / 50-100r / min to obtain an emulsified natural rubber latex.
[0109] A5. Weigh 0.108 kg of the stabilizer guaiacol, dissolve it in an equal proportion of hot water at 29° C., stir and mix evenly, disperse the diluted stabilizer in the emulsified natural rubber emulsion obtained in step A4, stir evenly at 30° C. at 30-60 s / 50-100 r / min to obtain a stabilized natural rubber emulsion.
[0110] A6. Weigh 0.054 kg of polyglycerol fatty acid ester as a dispersant, dissolve it in an equal proportion of 90° C. hot water, stir and mix evenly, disperse the diluted dispersant in the stabilized natural rubber emulsion obtained in step A5, stir evenly at 30° C. at 30-60S / 50-100r / min to obtain a dispersed natural rubber emulsion.
[0111] A7. Weigh 3.85 kg of bisphenol A, dissolve it in an equal proportion of 40° C. hot water, stir and mix evenly, disperse the diluted toughening agent in the dispersed natural rubber latex obtained in step A6, stir evenly at 30° C. at 30-60S / 50-100r / min, and compound with the dispersant to obtain the modified natural rubber latex.
[0112] A8. Demulsification and flocculation: Stir the above emulsion at high speed for 500-1000r / 2-10min to flocculate.
[0113] A9. Crepe sheets: The flocculated composite micelles (flocs) are creped using a crepe press.
[0114] A10. Washing: Put the crepe sheets into a washing tank and wash them with water.
[0115] A11. Granulation: Put the washed crepe sheets into the granulator for granulation;
[0116] A12. Dehydration and drying: After the granulated WF modified rubber is dehydrated, it is placed in a drying chamber at 60-90℃ and dried for 4-6 hours.
[0117] A13. The finished product after drying is toughened and modified natural rubber latex, which is then subjected to full physical and chemical performance testing.
[0118] The needle-resistant toughened modified natural rubber latex products obtained in Examples 1 to 5, as well as the control group 1 (conventional toughening agent) and blank WF were subjected to full physical and chemical test performance characterization. The reaction substances and parameters of the control group 1 were the same as those of Example 1, except that the toughening agent used therein was the conventional toughening agent bisphenol A. The specific tests were as follows:
[0119] 1.1 Technical indicators that characterize toughness include:
[0120] (1) Breaking strength; (2) Tensile stress; (3) Rebound elasticity and other indicators
[0121] The toughness of rubber is an important indicator to measure its ability to resist deformation due to external forces, mainly including tear strength and tensile stress. Tear strength, also known as tensile strength, refers to the load borne by the rubber per unit cross section when it is stretched to fracture, and the unit is megapascal (MPa). This indicator reflects the mechanical strength of the rubber during the stretching process. The larger the value, the better the strength of the rubber. Tensile stress, formerly known as tensile strength, refers to the load borne by the unit area when the rubber is stretched to a certain length. Commonly used tensile stresses are 100%, 300% and 500%. It reflects the ability of the rubber to resist deformation due to external forces. The larger the value, the better the toughness of the rubber, indicating that this type of rubber is less likely to produce elastic deformation. In addition, the physical and mechanical properties of rubber also include tensile strength, tear strength, elongation, permanent deformation, resilience, hardness and other indicators. These indicators together describe the comprehensive performance of the rubber, including its elasticity, strength, wear resistance and other aspects. Among them, tear strength and tensile stress are important indicators directly related to rubber toughness.
[0122] 1.2 The equipment used for testing is:
[0123] Internal mixer 1L / open mixer / flat vulcanizing press / tensile testing machine / Mooney viscometer / durometer / density meter / rebound tester / Akron abrader / DIN rotating roller abrader / plasticity meter / constant temperature blast drying oven / high temperature furnace.
[0124] Table 1 Basic formula of each test rubber compound
[0125]
[0126] Note: (a) Curing conditions: 140℃×30min, to make a curing test piece; (b) The number of recipes in Table 2 can be magnified.
[0127] 1.3 Test items and implementation standards
[0128] a). Volatile matter according to GB / T24131.1-2018
[0129] b). Ash content according to GB / T4498.1-2013
[0130] c). Nitrogen content according to GB / T8088-2008
[0131] d). Impurity content according to GB / T8086-2019
[0132] e). Initial plasticity value according to GB / T3510-2023
[0133] f). Plasticity retention rate GB / T3517-2022
[0134] g). Mooney viscosity ML100℃(1+4) according to GB / T 1232.1-2016;
[0135] h). Tensile strength, elongation at break, 100%, 300%, and tensile stress shall comply with GB / T528-2009;
[0136] i). Permanent deformation according to GB / T528-2009;
[0137] j). Tear strength according to GB / T529-2008;
[0138] k). Hardness (Shore A) according to GB / T 531.1-2008;
[0139] l). Density g / cm 3 According to GB / T533-2008;
[0140] m). Akron wear cm 3 According to GB / T 1689-2014;
[0141] n). DIN rotating roller wear mm 3 According to GB / T9867-2008;
[0142] o). Resilience % according to GB / T1681-2009;
[0143] Table 3 Mechanical properties test results of each rubber compound
[0144]
[0145] 1.4. Test results: It can be concluded from the performance test results in Table 3, the data results of the blank group and the control group 1 that the needle-resistant and toughened modified natural rubber latex product prepared by the present invention, the rubber compound mixed by the liquid in-situ method, has significantly improved physical comprehensive properties whether used alone or in combination with other rubber compounds or fillers, especially the tensile properties, tearing and wear resistance of the rubber compound are significantly improved compared with the blank WF rubber and bisphenol A (control group 1).
[0146] In addition, by adding the above-mentioned modified needle-resistant and toughened modified natural rubber latex liquid in-situ natural rubber into the formula of all-steel radial load-bearing tires and semi-steel passenger tires, the tire's durability, mileage, needle-puncture resistance, low rolling resistance, anti-skid and other performances are significantly improved, which complies with the EU tire labeling law.
[0147] The compounded toughened needle-resistant WF modified natural rubber of the present invention and its preparation method and application, the performance of the modified WF modified natural rubber of the present invention, in addition to maintaining the original physical properties, its biggest feature is needle-resistant, super toughness, tear resistance and prevention of flower breakage and block falling; this is confirmed by physical tests. In the WF modified natural rubber formula, natural mulberry branch extract DNJ (1-deoxynojirimycin) is used as modified natural rubber, which is directly added to natural rubber latex, and a compounded toughened needle-resistant modified natural rubber latex is produced by a compounding method.
[0148] Compared with the traditional WF natural rubber, the present invention uses guaiacol homologues and pure natural mulberry branch extract DNJ (1-deoxynojirimycin) as natural rubber latex synergistic modifiers, contains multiple biologically active ingredients, polyhydroxy alkaloids, such as carbohydrates, fatty acids, cellulose and polysaccharides, etc., and can achieve demulsification and flocculation of natural rubber latex without adding flocculants. Since flocculants such as acid and salt are not added, water washing is not required, thereby reducing water pollution. The overall preparation process is simple, the energy consumption is low, and it can be directly processed and produced on the basis of the original production line, and industrial production can be realized.
[0149] The above is only an embodiment of the present invention. For example, the toughening agent is specifically DNJ (1-deoxynojirimycin) C6H 13 NO4 white powder can realize the compound toughened and needle-resistant WF modified natural rubber of the present invention and its preparation method and application.
[0150] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.
Claims
1. A compound toughened and needle-resistant WF modified natural rubber, characterized in that: The components include the following by weight: natural rubber latex, diluent, emulsifier, dispersant, toughening agent; the dry content of the natural rubber latex is 25%-42%, the diluent is an aqueous ammonia solution with a mass fraction of 0.50%-5.00%, and the added amount of the diluent is 10%-80% of the dry content of the natural rubber latex; The emulsifier is an emulsifier of one or more long-chain compounds in a straight chain or branched chain containing 15 to 25 carbon atoms; the amount of the emulsifier added is 0.02% to 1.50% of the dry content of the natural rubber latex; The dispersant is a dispersant of one or more compounds containing 2-16 carbon atoms in a straight chain or branched chain; the added amount of the dispersant is 0.02%-0.90% of the dry content of the natural rubber latex; The toughening agent is a modifier of a straight chain or branched compound containing 5 to 10 carbon atoms, and the toughening agent is a pure natural mulberry branch extract DNJ; the toughening agent is added in an amount of 2.00% to 10.00% of the dry content of the natural rubber latex.
2. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 1, characterized in that: The toughening agent is specifically DNJ (1-deoxynojirimycin) C6H 13 NO4 white powder.
3. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 1, characterized in that: The emulsifier is specifically any one or two of long-chain octylphenol polyoxyethylene ether, dodecyltrimethylammonium chloride, polyglycerol fatty acid ester, and fatty acid polyglycerol ester.
4. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 2, characterized in that: The invention also comprises a stabilizer, which is any one of guaiacol, cresol, methylcresol and o-ethylphenol.
5. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 4, characterized in that: The stabilizer is guaiacol extracted from pine tar oil.
6. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 1, characterized in that: The dispersant is any one of erucamide, polyglycerol fatty acid ester, polyvinyl alcohol, vinyl alcohol copolymer, vinyl acetate-maleic anhydride copolymer and polyacrylic acid.
7. The method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to claim 1, characterized in that: The natural rubber latex is fresh latex newly cut from rubber trees, or ammonia-added natural rubber latex.
8. A method for preparing a compound toughened and needle-resistant WF-modified natural rubber according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) diluting the natural rubber latex with a diluent; diluting the natural rubber latex with the diluent to a concentration of 20%-40%, stirring evenly at a temperature of 20°C-60°C, at 30-60S / 50-100r / min, to obtain a natural latex dilution; (2) in a weakly alkaline state, preparing an emulsifier of a certain concentration, dispersing the emulsifier in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 70° C. at a temperature of 30 to 60 seconds and 50 to 100 revolutions per minute to obtain an emulsified natural rubber latex; Dispersing the stabilizer in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 60° C. at a temperature of 30 to 60 seconds and 50 to 100 revolutions per minute to obtain a stabilized natural rubber latex; (3) mixing the toughening agent and the dispersant with the natural rubber latex obtained in step (2); stirring and compounding at a temperature of 20° C. to 60° C.; Dispersing the dispersant in the natural rubber latex dilution obtained in step (1), stirring at a temperature of 20° C. to 60° C. for 30 to 60 seconds and 50 to 100 revolutions per minute to obtain a dispersed natural rubber latex; Dispersing the toughening agent in the natural rubber latex dilution obtained in step (1), stirring at high speed for 1 min-5 min / 500-1000 r / min at room temperature, to obtain a modified natural rubber latex; (4) After the reaction is completed, demulsification and flocculation are carried out, and the composite micelles (flocs) after flocculation are creped, washed, hammer-milled and granulated to obtain the finished product after drying, thereby obtaining a needle-resistant and toughened modified natural rubber latex.
9. An application of a compound toughened and needle-resistant WF-modified natural rubber, characterized in that: The compounded toughened and needle-resistant WF-modified natural rubber according to any one of claims 1 to 8 is used in tire manufacturing.