Modified acrylic resin, preparation method and application of modified acrylic resin in molding of soft porcelain material

Through the combination of aqueous acrylic resin, epoxy resin and cellulose nanocrystals, the problem of insufficient wear resistance and hydrophobicity of soft porcelain materials is solved, and low-cost and environmentally friendly preparation of modified acrylic resin is achieved, suitable for soft porcelain materials Wear and water resistance requirements.

CN118909376APending Publication Date: 2024-11-08GUANGXI UNIV FOR NATITIES +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411042841.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

Smart Images

  • Figure CN118909376A_ABST
    Figure CN118909376A_ABST
Patent Text Reader

Abstract

The invention discloses modified acrylic resin, a preparation method and application of the modified acrylic resin in soft porcelain material molding, and belongs to the technical field of modified acrylic resin.The modified acrylic resin is prepared from 16-24 parts of acrylic resin, 0.2-0.6 part of epoxy resin and 0.1-0.5 part of cellulose nanocrystals, the modified acrylic resin is prepared by mixing acrylic resin, epoxy resin and cellulose nanocrystals and then stirring at room temperature. The modified acrylic resin disclosed by the invention has excellent mechanical properties, hydrophobicity and hardness, the viscosity range is 390.2-483.6 cP, and the modified acrylic resin has a very good application prospect in soft porcelain material molding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of modified acrylic resins, and in particular relates to a modified acrylic resin, a preparation method and application thereof in soft porcelain material molding. Background Art

[0002] The existing traditional building materials mainly include stone, soil, etc. These are non-renewable resources. Excessive exploitation and use will lead to resource shortages. The production process consumes a lot of water and electricity energy and requires sewage discharge, which will also cause certain harm to the environment. The construction environment is bad and too much dust is generated, which will not only cause air pollution but also easily cause respiratory infections and affect health. Therefore, high-energy-consuming and high-pollution traditional products such as exterior wall tiles, mosaics, and clay panels are being eliminated. Therefore, the field of soft porcelain building materials has a very promising market.

[0003] Soft porcelain is a new type of soft wall decoration material that can replace ceramic tiles, mosaics, marble and other soft materials. Soft porcelain is made by processing modified inorganic powder and water-based polymer emulsion. The quality of water-based polymer emulsion directly affects the quality of soft porcelain. In practical applications, soft porcelain materials are soft and elastic, so they are more wear-resistant. In order to improve the service life and water resistance of soft porcelain materials, it is necessary to develop coatings with good mechanical properties, strong hydrophobicity, strong adhesion and good wear resistance. The existing water-based acrylic emulsion has the advantages of environmental protection and good adhesion, but the waterproof performance and wear resistance cannot meet the requirements.

[0004] Chinese patent CN201610909112.8 discloses a modified acrylic coating, its preparation method and application. The modified acrylic coating includes a modified acrylic emulsion, an additive and water. The modified acrylic emulsion is compounded by a synthetic emulsion and a wax emulsion. It has the advantages of strong adhesion after film formation, and has excellent water repellency, water resistance and wear resistance. However, the patent uses a large number of additives including film additives, dispersants, defoamers, thickeners, wetting agents and leveling agents, which increases the production and processing costs.

[0005] Chinese patent CN201811383937.6 discloses a water-based self-crosslinking acrylic self-drying coating and its preparation method, which improves the crosslinking density of acrylic emulsion by introducing ethyl acetoacetate methacrylate self-crosslinking monomer and utilizing the crosslinking curing characteristics of the monomer. However, ketone hydrazine crosslinking is affected by many factors such as pH and temperature, and the improvement in the performance of soft porcelain is not significant.

[0006] Chinese patent CN112029453A discloses a preparation technology of an adhesive with polyurethane as the main material. Through the chemical reaction between polyurethane, epoxy resin and acrylate, an interpenetrating network structure polymer is formed, which greatly improves its mechanical properties, but does not solve the problems of hydrophobicity, adhesion and hardness. According to literature research and actual industrial production investigation, polyurethane is expensive and is not suitable for soft porcelain.

[0007] Chinese patent CN202310075814.0 discloses that the present invention mainly uses carboxyl-type aqueous emulsion as the main material, and prepares the performance of two or more emulsions through emulsion mixing technology to optimize the coating performance. On this basis, a carboxyl-type cross-linking agent is introduced to achieve mixed cross-linking of soft and hard emulsions to form an interpenetrating network structure and improve molecular cohesion, but its mechanical properties are not suitable for the preparation of soft magnetic sheets. Summary of the invention

[0008] The purpose of the present invention is to provide a modified acrylic resin, a preparation method and its application in soft porcelain material molding to solve the technical problems of high energy consumption, high pollution, low wear resistance, high cost and low mechanical properties in the above-mentioned prior art. The modified acrylic resin product prepared by the present invention does not add film additives, dispersants, defoamers, thickeners, wetting agents and leveling agents and has excellent mechanical properties, hydrophobicity and hardness.

[0009] In order to achieve the above object, the technical solution of the present invention is as follows:

[0010] A modified acrylic resin, comprising the following components in parts by mass:

[0011] 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin, and 0.1-0.5 parts of cellulose nanocrystals.

[0012] Furthermore, the acrylic resin is a water-based acrylic resin.

[0013] Furthermore, the acrylic resin is in liquid state, and has a viscosity ranging from 340 to 360 cP.

[0014] Furthermore, the epoxy resin is in liquid state, and has a viscosity ranging from 60 to 80 cP.

[0015] Furthermore, the cellulose nanocrystals are in liquid state with a viscosity ranging from 1 to 10 cP.

[0016] Furthermore, the water-based acrylic resin is prepared by solution polymerization from methyl methacrylate, butyl acrylate, styrene, methacrylic acid, acrylamide, glycidyl methacrylate, silane coupling agent, sodium allyloxyhydroxypropyl sulfonate, alkyl polyoxyethylene ether, disodium lauryl sulfosuccinate ethoxylate, and ammonium persulfate.

[0017] Furthermore, the preparation method of the water-based acrylic resin comprises the following steps:

[0018] (1) adding 100-120 parts of methyl methacrylate, 80-100 parts of butyl acrylate, 10-15 parts of styrene, 2-5 parts of methacrylic acid, 5-8 parts of acrylamide, 2-5 parts of glycidyl methacrylate, 2-5 parts of silane coupling agent, 1-3 parts of sodium allyloxyhydroxypropyl sulfonate, and 1-3 parts of alkyl polyoxyethylene ether in sequence, by parts by mass, to prepare an emulsion for use;

[0019] (2) adding 4-6 g of deionized water and 4-6 g of anionic emulsifier ethoxylated sulfosuccinate monolaurate disodium salt as a base solvent, and when the temperature rises to 83-85° C., adding 10-15 g of the emulsion prepared in step (1) and 0.1-0.3 g of initiator ammonium persulfate, and reacting for 10-15 min;

[0020] (3) adding the remaining emulsifier prepared in step (1) until the reaction is completed, with a dripping flow rate of 100-120 g / h, cooling to 65-70° C., and simultaneously dripping 0.1-0.3 g of an oxidant and 0.05-0.15 g of a reducing agent, dripping for 20-25 min, and then keeping the temperature for 10-15 min, adjusting the pH to 7.5-8.5, cooling the temperature to room temperature 25° C., and then filtering with a filter cloth to obtain a water-based acrylic resin.

[0021] The preparation reaction equation of the water-based acrylic acid resin is as follows:

[0022]

[0023] The invention also provides a method for preparing the modified acrylic resin, which comprises mixing 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin and 0.1-0.5 parts of cellulose nanocrystals, and stirring the mixture at room temperature to obtain the modified acrylic resin.

[0024] Further, the modified acrylic resin is prepared by stirring at room temperature and 600-700 r / min for 2-3 hours.

[0025] The invention also provides an application of modified acrylic acid, which is applied to the molding of soft porcelain materials.

[0026] Compared with the prior art, the present invention has the following technical advantages:

[0027] 1. The modified acrylic resin of the present invention uses water-based epoxy resin and cellulose nanocrystals as filling particles added to the resin. EP reacts with the synthetic acrylic resin to generate a large number of hydroxyl groups (-OH). The epoxy resin modification can improve the shortcomings of acrylic adhesives such as poor water resistance, weak adhesion, brittleness at low temperatures, and viscosity and loss of strength at high temperatures.

[0028] 2. The present invention uses CNC as filling particles to provide skeleton support for the coating while increasing reasonable roughness, thereby significantly improving mechanical properties, hydrophobicity, adhesion and hardness.

[0029] 3. The preparation process of the present invention is simple, the cost is low, there is no VOC emission, it is energy-saving and environmentally friendly, and it is convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the reaction flow chart of the present invention.

[0031] Figure 2 The figure is a relationship diagram between the viscosity of the modified acrylic resin prepared by the present invention and the content of the waterborne epoxy resin.

[0032] Figure 3 The figure is a relationship diagram between the tensile strength of the modified acrylic resin prepared by the present invention and the content of cellulose nanocrystals.

[0033] Figure 4 The figure is a relationship diagram between the tensile strength and temperature of the modified acrylic resin prepared by the present invention. DETAILED DESCRIPTION

[0034] To further explain the technical means and effects of the present invention, the technical solution of the present invention is further described below in conjunction with the embodiments of the present invention, but the present invention is not limited to the scope of the embodiments.

[0035] In an embodiment of the present invention, a modified acrylic resin comprises the following components in parts by mass:

[0036] 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin, and 0.1-0.5 parts of cellulose nanocrystals.

[0037] The acrylic resin is a water-based acrylic resin.

[0038] The acrylic resin is in liquid state and has a viscosity range of 340-360 cP.

[0039] The epoxy resin is in liquid state and has a viscosity range of 60-80 cP.

[0040] The cellulose nanocrystals are in liquid state and have a viscosity range of 1-10 cP.

[0041] like Figure 1 As shown, the preparation method of the water-based acrylic resin comprises the following steps:

[0042] (1) adding 100-120 parts of methyl methacrylate, 80-100 parts of butyl acrylate, 10-15 parts of styrene, 2-5 parts of methacrylic acid, 5-8 parts of acrylamide, 2-5 parts of glycidyl methacrylate, 2-5 parts of silane coupling agent, 1-3 parts of sodium allyloxyhydroxypropyl sulfonate, and 1-3 parts of alkyl polyoxyethylene ether in sequence, by parts by mass, to prepare an emulsion for use;

[0043] (2) adding 4-6 g of deionized water and 4-6 g of anionic emulsifier ethoxylated sulfosuccinate monolaurate disodium salt as a base solvent, and when the temperature rises to 83° C., adding 10-15 g of the emulsion prepared in step (1) and 0.1-0.3 g of initiator ammonium persulfate, and reacting for 10-15 min;

[0044] (3) adding the remaining emulsifier prepared in step (1) until the reaction is completed, with a dripping flow rate of 100-120 g / h, cooling to 65-70° C., and simultaneously dripping 0.1-0.3 g of an oxidant and 0.05-0.15 g of a reducing agent, dripping for 20-25 min, and then keeping the temperature for 10-15 min, adjusting the pH to 7.5-8.5, cooling the temperature to room temperature 25° C., and then filtering with a filter cloth to obtain a water-based acrylic resin.

[0045] The preparation method of the modified acrylic resin is to mix 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin and 0.1-0.5 parts of cellulose nanocrystals, and stir at room temperature and 600-700 r / min for 2-3 hours to obtain the modified acrylic resin.

[0046] In order to make the disclosure of the present invention more complete, it is described below through more specific embodiments.

[0047] Example 1

[0048] A method for preparing a modified acrylic resin comprises the following steps:

[0049] S1. Preparation of acrylic resin:

[0050] (1) In a round-bottom flask, add 60 g of MMA, 80 g of BA, 6 g of ST, 5 g of MAA, 6 g of AM, 1 g of GMA, 1 g of A-1711 g, 0.5 g of COPS-1, 0.5 g of LCN-118, and 40 g of deionized water in sequence to prepare 200 g of emulsion for use.

[0051] (2) Add 30g of deionized water and 1g of anionic emulsifier DES-330 as the base solvent. When the experimental temperature rises to 83°C, add 10g of the prepared emulsion and 0.2g of initiator APS and react for 10min. Add the remaining 190g of emulsifier (drop flow rate 100g / h) until the reaction is completed. Cool down to 65°C, and at the same time, drop 0.2g of oxidant tert-butyl hydroperoxide and 0.1g of FF6M formaldehyde-free reducing agent. Add for 20min, keep warm for 10min, and adjust the pH to 8.5. Cool the four-necked flask to room temperature, and then filter with a 200-mesh filter cloth to obtain acrylic resin.

[0052] S2. Preparation of modified acrylic resin: 20 g acrylic resin and 0.4 g epoxy resin were added into a conical flask in sequence, and stirred at room temperature and 600-700 r / min for 3 h.

[0053] The following single factor experiment is used to optimize the preparation process of modified acrylic resin:

[0054] (1) Study on the effect of different epoxy resin contents on adhesive viscosity

[0055] The preparation method of the modified acrylic resin is basically the same as that of Example 1, except that 0.4 g, 1 g, 2 g, 3 g, and 5 g of epoxy resin are added to 20 g of acrylic resin, and the corresponding viscosities are measured to investigate the effect of different epoxy resin contents on the viscosity of the adhesive. The results are shown in FIG. Figure 2 ,Depend on Figure 2 It can be seen that with the increase of the amount of epoxy resin added, the viscosity of the emulsion increases, but too high an emulsion viscosity will lead to poor fluidity of the emulsion, which is not conducive to the preparation of soft magnetic sheets. Therefore, when 0.4g of epoxy resin is added, the emulsion viscosity is most suitable.

[0056] (2) Effects of different cellulose nanocrystals on tensile strength

[0057] The preparation method of the modified acrylic resin is basically the same as that of Example 1, except that 0.4 g of epoxy resin is added to 20 g of acrylic resin, and then 0.2 g, 0.3 g, 0.4 g, 0.5 g, and 0.9 g of cellulose nanocrystals are added to measure the corresponding tensile strength, and the effect of different cellulose nanocrystal contents on the tensile strength is investigated. The results are shown in FIG. Figure 3 ,Depend on Figure 3 It can be seen that as the content of cellulose nanocrystals increases, the tensile strength first increases and then decreases. When the cellulose nanocrystals are 0.3g, the tensile strength is the largest, so the cellulose nanocrystals are optimal when they are 0.3g.

[0058] (3) Effect of different reaction temperatures on tensile strength

[0059] The preparation method of the modified acrylic resin is basically the same as that of Example 1, except that 0.4 g of epoxy resin and 0.3 g of cellulose nanocrystals are added to 20 g of acrylic resin, and the influence of different reaction temperatures (25°C, 35°C, 45°C, 55°C, 65°C) on the tensile strength is measured. The influence of different reaction temperatures on the tensile strength is investigated. The results are shown in FIG. Figure 4 ,Depend on Figure 4 It can be seen that as the reaction temperature increases, the tensile strength decreases continuously, so 25°C is the best choice.

[0060] Example 2

[0061] A method for preparing a modified acrylic resin comprises the following steps:

[0062] S1. Preparation of acrylic resin: Add 60 g MMA, 80 g BA, 6 g ST, 5 g MAA, 6 g AM, 1 g GMA, 1 g A-1711 g, 10.5 g COPS-1, 0.5 g LCN-118, 40 g deionized water and other monomers to a round-bottom flask to prepare 200 g of emulsion for use. Add 30 g deionized water and 1 g anionic emulsifier DES-330 as the base solvent. When the experimental temperature rises to 83 ° C, add 10 g of the prepared emulsion and 0.2 g initiator APS, and react for 10 min. Add the remaining 190 g emulsifier (drop flow rate 100 g / h) until the reaction is completed. Cool down to 65 ° C, and at the same time, drop 0.2 g oxidant tert-butyl hydroperoxide and 0.1 g FF6M formaldehyde-free reducing agent, add for 20 min, keep warm for 10 min, and adjust the pH to 8.5. The four-necked flask was cooled to room temperature, and then filtered through a 200-mesh filter cloth to obtain an acrylic resin.

[0063] S2. Preparation method of modified acrylic resin: 20 g acrylic resin, 0.4 g epoxy resin and 0.2 g cellulose nanocrystals are added into a conical flask in sequence, and stirred at room temperature (25° C.) and 600-700 r / min for 3 h.

[0064] Example 3

[0065] A method for preparing a modified acrylic resin comprises the following steps:

[0066] S1. Preparation of acrylic resin: Add 60 g MMA, 80 g BA, 6 g ST, 5 g MAA, 6 g AM, 1 g GMA, 1 g A-1711 g, 10.5 g COPS-1, 0.5 g LCN-118, 40 g deionized water and other monomers to a round-bottom flask to prepare 200 g of emulsion for use. Add 30 g deionized water and 1 g anionic emulsifier DES-330 as the base solvent. When the experimental temperature rises to 83 ° C, add 10 g of the prepared emulsion and 0.2 g initiator APS, and react for 10 min. Add the remaining 190 g emulsifier (drop flow rate 100 g / h) until the reaction is completed. Cool down to 65 ° C, and at the same time, drop 0.2 g oxidant tert-butyl hydroperoxide and 0.1 g FF6M formaldehyde-free reducing agent, add for 20 min, keep warm for 10 min, and adjust the pH to 8.5. The four-necked flask was cooled to room temperature, and then filtered through a 200-mesh filter cloth to obtain an acrylic resin.

[0067] S2. Preparation method of modified acrylic resin: 20 g acrylic resin, 0.4 g epoxy resin and 0.4 g cellulose nanocrystals are added into a conical flask in sequence, and stirred at room temperature (25° C.) and 600-700 r / min for 3 h.

[0068] Example 4

[0069] A method for preparing a modified acrylic resin comprises the following steps:

[0070] S1. Preparation of acrylic resin: Add 60 g MMA, 80 g BA, 6 g ST, 5 g MAA, 6 g AM, 1 g GMA, 1 g A-1711 g, 10.5 g COPS-1, 0.5 g LCN-118, 40 g deionized water and other monomers to a round-bottom flask to prepare 200 g of emulsion for use. Add 30 g deionized water and 1 g anionic emulsifier DES-330 as the base solvent. When the experimental temperature rises to 83 ° C, add 10 g of the prepared emulsion and 0.2 g initiator APS, and react for 10 min. Add the remaining 190 g emulsifier (drop flow rate 100 g / h) until the reaction is completed. Cool down to 65 ° C, and at the same time, drop 0.2 g oxidant tert-butyl hydroperoxide and 0.1 g FF6M formaldehyde-free reducing agent, add for 20 min, keep warm for 10 min, and adjust the pH to 8.5. The four-necked flask was cooled to room temperature, and then filtered through a 200-mesh filter cloth to obtain an acrylic resin.

[0071] S2. Preparation method of modified acrylic resin: 20 g acrylic resin, 0.4 g epoxy resin and 0.3 g cellulose nanocrystals are added into a conical flask in sequence, and stirred at 25° C. and 600-700 r / min for 2 h.

[0072] Test Example

[0073] The modified acrylic resins prepared in Examples 1-4 were subjected to performance tests, including hydrophobicity, hardness, mechanical properties, and viscosity tests, and the test methods were as follows:

[0074] 1. Hydrophobic performance test

[0075] The static water contact angle of the latex coating on the glass plate was analyzed by the sessile drop method at 25° C. The average value of the angles obtained at more than 10 different positions on each sample surface was taken.

[0076] 2. Hardness performance test

[0077] The pencil hardness of modified acrylic resin was measured according to ISO15184:2012 standard.

[0078] 3. Mechanical properties test

[0079] According to the national standard GB / T 528-2009 "Tensile stress-strain properties of vulcanized rubber or thermoplastic rubber

[0080] According to the requirements of "Determination of Energy", first cut out a sample with a size of 20mm×10mm (thickness 2-3mm), debug the tensile testing machine, and conduct a tensile test experiment at a rate of 100±10mm / min to obtain and analyze the data.

[0081] 4. Viscosity test

[0082] Refer to GB / T 2794-2022 and GB / T 7193-2008 for viscosity test requirements. Use Brookfield digital viscometer to measure the viscosity of modified acrylic resin at 25°C.

[0083] Experimental data of each embodiment:

[0084] Table 1 Experimental data of the embodiment

[0085]

[0086] It can be seen from the data in Table 1 that the modified acrylic resin prepared by the present invention has excellent mechanical properties, hydrophobicity and hardness, a viscosity range of 390.2-483.6 cP, and a simple preparation process, low cost, no VOC emissions, energy saving and environmental protection, easy industrial production, and has a good application prospect in soft porcelain material molding.

[0087] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A modified acrylic resin, characterized in that: By mass, it contains the following components: 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin, and 0.1-0.5 parts of cellulose nanocrystals.

2. A modified acrylic resin as claimed in claim 1, characterized in that: The acrylic resin is a water-based acrylic resin.

3. A modified acrylic resin as claimed in claim 2, characterized in that: The water-based acrylic resin is prepared by solution polymerization from methyl methacrylate, butyl acrylate, styrene, methacrylic acid, acrylamide, glycidyl methacrylate, silane coupling agent, sodium allyloxyhydroxypropyl sulfonate, alkyl polyoxyethylene ether, disodium lauryl sulfosuccinate ethoxylate and ammonium persulfate.

4. A modified acrylic resin as claimed in claim 3, characterized in that: The preparation method of the water-based acrylic resin comprises the following steps: (1) adding 100-120 parts of methyl methacrylate, 80-100 parts of butyl acrylate, 10-15 parts of styrene, 2-5 parts of methacrylic acid, 5-8 parts of acrylamide, 2-5 parts of glycidyl methacrylate, 2-5 parts of silane coupling agent, 1-3 parts of sodium allyloxyhydroxypropyl sulfonate, and 1-3 parts of alkyl polyoxyethylene ether in sequence, by parts by mass, to prepare an emulsion for use; (2) adding 4-6 g of deionized water and 4-6 g of anionic emulsifier ethoxylated sulfosuccinate monolaurate disodium salt as a base solvent, and when the temperature rises to 83-85° C., adding 10-15 g of the emulsion prepared in step (1) and 0.1-0.3 g of initiator ammonium persulfate, and reacting for 10-15 min; (3) adding the remaining emulsifier prepared in step (1) until the reaction is completed, with a dripping flow rate of 100-120 g / h, cooling to 65-70° C., and simultaneously dripping 0.1-0.3 g of an oxidant and 0.05-0.15 g of a reducing agent, dripping for 20-25 min, and then keeping the temperature for 10-15 min, adjusting the pH to 7.5-8.5, cooling the temperature to room temperature 25° C., and then filtering with a filter cloth to obtain a water-based acrylic resin.

5. A modified acrylic resin as claimed in claim 1, characterized in that: The acrylic resin is in liquid state and has a viscosity range of 340-360 cP.

6. A modified acrylic resin as claimed in claim 1, characterized in that: The epoxy resin is in liquid state and has a viscosity range of 60-80 cP.

7. A modified acrylic resin as claimed in claim 1, characterized in that: The cellulose nanocrystals are in liquid state and have a viscosity range of 1-10 cP.

8. A method for preparing a modified acrylic resin according to any one of claims 1 to 7, characterized in that: The method is prepared by mixing 16-24 parts of acrylic resin, 0.2-0.6 parts of epoxy resin and 0.1-0.5 parts of cellulose nanocrystals, and stirring the mixture at room temperature.

9. The method for preparing the modified acrylic resin according to claim 8, characterized in that: The modified acrylic resin was prepared by stirring at room temperature and 600-700 r / min for 2-3 hours.