Self-dissolving antibacterial hydrogel as well as preparation method and application thereof
The self-dissolving antibacterial hydrogel regulated by silver nanoparticles achieves the self-dissolving transformation of the hydrogel at room temperature, enhancing its mechanical properties and antibacterial activity, and is suitable for medical, food, and construction fields.
Patent Information
- Application Number
- CN202410984196.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hydrogels are difficult to transform from gels to sols under mild conditions, and traditional methods require the participation of catalysts or enzymes, which affects the regulation of their flexibility and sustained-release properties.
A self-dissolving antibacterial hydrogel is used, with silver nanoparticles as sol-gel inducing agents to regulate the interaction of the polymer interpenetrating network, achieving the transformation of the hydrogel from gel to sol at room temperature without the need for catalysts or enzymes.
The self-dissolution of hydrogels at room temperature enhances mechanical properties and antibacterial properties, solving the problem of regulating the flexibility and sustained-release properties of hydrogels under mild conditions, and making it suitable for medical, food, and construction fields.
Smart Images

Figure CN118909380A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials, and specifically relates to a self-dissolving antibacterial hydrogel and a preparation method and application thereof. Background Art
[0002] Hydrogel is a material formed by swelling of a three-dimensional polymer network with high water content in water. Hydrogels can be divided into natural polymer hydrogels and synthetic hydrogels according to the source of the polymer. Natural polymer hydrogels have good biocompatibility and a wide range of sources. Due to the complex and poor reproducibility of their synthesis process, they are difficult to modify in terms of strength, flexibility and chemical properties. Synthetic hydrogels are more flexible in mechanical properties and functional control, and can be given specific physical and chemical properties by regulating the structure of the molecular chain. Therefore, more and more scholars have paid attention to them. In the past few decades, hydrogels have been widely used in many fields such as medical antibacterial, drug delivery, cosmetics, and preservatives due to their advantages such as adjustable water retention, sustained release and biocompatibility, and have achieved good results. Traditional hydrogels have low strength and lack of good flexibility, which limits their use as special functional materials to solve problems in medicine, engineering and food safety. Therefore, in the past few decades, scientists' research on gels has mainly focused on the regulation of their mechanical properties. From a molecular perspective, hydrogels formed based on a single chemical bond or interacting polymer network have deficiencies in mechanical strength, stretchability, and fatigue resistance. Based on the rheological properties of polymer materials, the modification of the molecular chain topological structure and interaction force can improve the mechanical properties of hydrogels, such as mechanical strength, stretchability, and fatigue resistance, such as topological hydrogels and double-network hydrogels.
[0003] Although this type of hydrogel is a polymer network composed of chemically cross-linked rigid segments, crystalline structures or glassy segments, and exhibits excellent mechanical properties and stable rheological properties under mild conditions, an overly stable polymer network is not conducive to the regulation of sustained release, and this type of hydrogel as a base material for coatings and dressings also has the disadvantages of too strong adhesion and inability to achieve non-destructive peeling, which can cause secondary damage to the protected material. A feasible solution is to make the hydrogel degradable or undergo a sol-gel transformation over time. It is usually necessary to introduce specific catalysts and sustained-release agents to destroy specific chemical bonds in the hydrogel network, such as catalytic hydrolysis or enzymatic degradation to achieve the breakage of ester and amide molecular chains. This catalysis of the polymer main chain requires the introduction of components for breaking the main chain into the hydrogel system and has high requirements for catalytic conditions, and is not suitable for regulating the rheological properties of hydrogels under mild conditions. Therefore, in order to achieve the transformation of hydrogels from gel to sol at room temperature, a new gel still needs to be developed. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention provides a self-dissolving antibacterial hydrogel, which uses a solubilization inducer to regulate the interaction of the polymer interpenetrating network in the hydrogel, and can achieve the disintegration of the cross-linked polymer network in the hydrogel without introducing a catalyst or enzyme, that is, without resorting to chemical reactions, and realize the transformation of the hydrogel from a gel to a sol at room temperature.
[0005] The invention also provides a method for preparing the self-dissolving antibacterial hydrogel.
[0006] The invention also provides an application of the self-dissolving antibacterial hydrogel.
[0007] A first aspect of the present invention provides a self-dissolving antibacterial hydrogel, wherein the self-dissolving antibacterial hydrogel comprises an interpenetrating network structure formed by a first polymer and a second polymer, wherein a solubilization inducer is distributed in the interpenetrating network structure, wherein the first polymer comprises polyacrylamide, the second polymer comprises at least one of sodium alginate, polyacrylic acid and polymethacrylic acid, and the solubilization inducer comprises silver nanoparticles.
[0008] One of the technical solutions of the present invention regarding the self-dissolving antibacterial hydrogel has at least the following beneficial effects:
[0009] The present invention utilizes a solization inducing agent to regulate the interaction of the polymer interpenetrating network in the hydrogel, and can achieve the disintegration of the cross-linked polymer network in the hydrogel without introducing a catalyst or enzyme, that is, without resorting to a chemical reaction, and can achieve the transformation of the hydrogel from a gel to a sol at room temperature. This hydrogel is of great significance not only for the rescue moisturizing and reinforcement of fragile materials, but also for promoting the application of hydrogels in the fields of medicine, food, construction, archaeology, etc.
[0010] When the solubilization inducer is silver nanoparticles, the hydrogel with rheological properties regulated by silver nanoparticles has good antibacterial properties. It can not only provide antibacterial protection as a dressing, but also solve the problem of bacterial growth during the preservation of the hydrogel itself.
[0011] The self-dissolving hydrogel of the present invention can be used as a base material for drug sustained release, chelation, and deacidification components. After being solvated, it is attached to the sample surface in the form of a coating. The problem of residual base material can be solved by simple cleaning, and the release of functional components such as drug sustained release, chelation, and deacidification can also be regulated during the solvation process.
[0012] In the self-dissolving hydrogel of the present invention, the first polymer provides a covalent cross-linking network for the hydrogel. The second polymer, such as sodium alginate, is a commonly used polymer containing carboxylic acid groups and is used to provide ionic cross-linking for the hydrogel.
[0013] The invention improves the preparation of nano silver, the nano silver is formed in a mixed system of sodium alginate and acrylamide, the heating link is reduced, the energy is saved, and the nano silver is evenly distributed inside the hydrogel.
[0014] The invention mixes nano silver with hydrogel to prepare nano silver antibacterial self-dissolving hydrogel, changes the cross-linking structure of the macromolecules inside the hydrogel, not only enhances the mechanical properties of the hydrogel, but also enables the hydrogel to have the self-dissolving property of solubilization over time.
[0015] The preparation method involved in the invention is simple, has strong controllability, can realize mass production, and has high practical value.
[0016] The self-dissolving antibacterial hydrogel of the invention has good tensile properties and can reach a tensile multiple of 100% to 2500%.
[0017] According to some embodiments of the present invention, the content of the silver nanoparticles in the hydrogel is 0.001 g / L to 10.00 g / L.
[0018] According to some embodiments of the present invention, the content of the silver nanoparticles in the hydrogel is any value among 0.01 g / L, 0.02 g / L, 0.03 g / L, 0.04 g / L, 0.05 g / L, 0.06 g / L, 0.07 g / L, 0.08 g / L, 0.09 g / L, 0.10 g / L, or a range formed by any two of them.
[0019] According to some embodiments of the present invention, the content of the silver nanoparticles in the hydrogel is any value among 0.1 g / L, 0.2 g / L, 0.3 g / L, 0.4 g / L, 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L, 1.0 g / L or a range formed by any two of them.
[0020] According to some embodiments of the present invention, the content of the silver nanoparticles in the hydrogel is any value among 1g / L, 2g / L, 3g / L, 4g / L, 5 / L, 6g / L, 7g / L, 8g / L, 9g / L, 10g / L or a range formed by any two of them.
[0021] According to some embodiments of the present invention, a functional component is further distributed in the self-dissolving antibacterial hydrogel, and the functional component includes at least one of a deacidifying agent and a chelating agent.
[0022] According to some embodiments of the present invention, the deacidification agent includes at least one of sodium bicarbonate, sodium hydroxide, calcium carbonate, calcium bicarbonate, magnesium oxide, sodium bicarbonate, sodium carbonate, potassium carbonate, potassium bicarbonate and calcium oxide. These inorganic salts or oxides of corresponding metals can be used as alternative deacidification components to reduce the surface acidity of the protected material.
[0023] According to some embodiments of the present invention, the chelating agent includes catechol, 1,10-phenanthroline, ethylenediaminetetraacetic acid (EDTA) and potassium and sodium salts thereof, and the chelating agent can replace the deacidification component to remove deposited salt and rust from the surface of the protected material.
[0024] According to some embodiments of the present invention, the functional component further comprises a drug having a therapeutic effect, and the purpose of sustained release can be achieved by doping the drug into the self-dissolving hydrogel system of the present invention.
[0025] The second aspect of the present invention provides a method for preparing the self-dissolving antibacterial hydrogel of the first aspect, comprising the following steps:
[0026] S1: mixing the first polymer monomer, the second polymer and the cross-linking agent and evacuating the mixture to obtain a precursor solution;
[0027] S2: adding a solvation inducing agent precursor and a reducing agent to the precursor solution, and stirring for the first time in the dark to obtain a first intermediate product;
[0028] S3: adding a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark for a second time, and then irradiating with ultraviolet light to obtain the self-dissolving antibacterial hydrogel; or, step S3 includes: adding a functional component, a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark, and then irradiating with ultraviolet light to obtain the self-dissolving antibacterial hydrogel.
[0029] A technical solution in the method for preparing the self-dissolving antibacterial hydrogel of the present invention has at least the following beneficial effects:
[0030] The preparation method of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.
[0031] The preparation method of the present invention uses ultraviolet light irradiation during the preparation process, does not require high temperature conditions, can complete the preparation of hydrogel at room temperature, and avoids the possibility of heat-sensitive substances being denatured or destroyed by heat. The use of a precursor solution can obtain a preliminary intermediate product through simple mixing, vacuum extraction and other steps, so that the preparation process is relatively efficient and the manufacturing cost is reduced. In the stage of the formation of the second intermediate product, by adding functional components, hydrophilicity regulators, initiators and catalysts, the release of functional components such as drug sustained release, chelation, deacidification in the hydrogel can be accurately regulated, thereby increasing the application flexibility of the hydrogel. Adding a solubilization inducer, such as silver nanoparticles, can effectively improve the antibacterial properties of the hydrogel.
[0032] Since self-dissolving antibacterial hydrogel not only has antibacterial properties, it can also be used in construction, food, archaeology and other fields, expanding its market potential and practical application scenarios.
[0033] The preparation method of the present invention does not require the use of a large amount of organic solvents or high-energy consumption equipment during the preparation process, is relatively environmentally friendly, and meets the sustainable development requirements of modern manufacturing.
[0034] According to some embodiments of the present invention, the mass ratio of the first polymer monomer to the second polymer is 1:3-10.
[0035] According to some embodiments of the invention, the first polymer monomer comprises acrylamide.
[0036] According to some embodiments of the present invention, the second polymer includes sodium alginate, which is a commonly used polymer containing carboxylic acid groups and is used to provide ionic crosslinking for hydrogels. It can also be replaced by polyacrylic acid or polymethacrylic acid, and its content in the polymerization reaction precursor is 0.1 wt% to 10 wt%.
[0037] According to some embodiments of the present invention, the crosslinking agent includes at least one of N,N'-methylenebisacrylamide, divinylbenzene, N,N'-(1,2-dihydroxyethylene)diacrylamide, ethylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate and triethylene glycol dimethacrylate.
[0038] The crosslinking agent contains at least two carbon-carbon double bonds, and together with the first polymer monomer (containing at least one carbon-carbon double bond), it initiates free radical polymerization to form a polymer spatial network (chemical crosslinking promotes gelation, but during the production of the molecular chain, there will also be physical crosslinking such as chain segment entanglement to form gelation). Regulating the concentration of the crosslinking agent can make the connection of this spatial network weaker, and as the physical crosslinking is destroyed under the action of the nanosilver particles, the hydrogel becomes solubilized.
[0039] According to some embodiments of the present invention, the amount of the cross-linking agent added is 0.01 wt% to 10.0 wt% of the sum of the mass of the first polymer monomer and the second polymer.
[0040] According to some embodiments of the present invention, the solvation inducing agent precursor comprises silver nitrate.
[0041] The ratio of silver nitrate to precursor solution is (0.001-0.003) g: (50-70) mL.
[0042] According to some embodiments of the present invention, the reducing agent includes citrate (such as sodium citrate), glucose, formaldehyde, tartrate, and nanocellulose, and its function is to react with silver nitrate to reduce monovalent silver into elemental silver and form silver nanoparticles through coordination.
[0043] According to some embodiments of the present invention, the mass ratio of the solvation inducing agent precursor to the reducing agent is 1:20-270.
[0044] In step S1, the first polymer monomer, the second polymer and the cross-linking agent are mixed and then vacuumed. The mixture may be stirred at 25-35° C. for 5-9 hours, and then vacuumed at 0.01 MPa for 3-5 hours.
[0045] In step S1, the first polymer monomer, the second polymer and the cross-linking agent are mixed and then vacuumed, and stirred at 25-28° C. for 6-8 hours.
[0046] In step S2, the second polymer sodium alginate is dissolved during the stirring process.
[0047] When the second polymer is sodium alginate, the ratio of sodium alginate to water is (1-2) g: (50-70) mL.
[0048] Water is deionized water and ultrapure water.
[0049] The sodium alginate is high viscosity sodium alginate, more preferably liquid phase sodium alginate.
[0050] The sodium alginate is a high-viscosity sodium alginate, and more preferably a liquid-phase sodium alginate, which is conducive to regulating the gelation time and the dispersion of the silver nanoparticles.
[0051] According to some embodiments of the present invention, the first light-protected stirring time is 20 min to 30 min.
[0052] According to some embodiments of the present invention, the first light-protected stirring time is 20 min to 25 min.
[0053] The first intermediate product is a solution containing monomers and silver nanoparticles, in which silver nitrate is converted into silver nanoparticles by sodium citrate on the basis of a precursor solution. The solution contains monomers and crosslinking agents containing carbon-carbon double bonds required for polymerization and can form a hydrogel by free radical polymerization.
[0054] According to some embodiments of the present invention, the second light-shielded stirring time is 20 s to 80 s.
[0055] According to some embodiments of the present invention, the second light-shielded stirring time is 20s to 25s.
[0056] According to some embodiments of the present invention, the functional component includes sodium bicarbonate, which can reduce the acidity of the surface of the protected material when the hydrogel is used as a dressing, thereby neutralizing the acidity. Other drugs can also be used instead for other applications, such as chelating agents, weak acids, etc., to remove stubborn inorganic salt deposits.
[0057] According to some embodiments of the present invention, the hydrophilicity regulator includes methacrylamide, which is a monomer used to replace acrylamide to change the hydrophilicity of the polymer network, thereby controlling the volume change of the hydrogel after reaching swelling equilibrium.
[0058] According to some embodiments of the present invention, the initiator includes potassium persulfate to initiate free radical polymerization, and may also be replaced by other initiators, such as ammonium persulfate, azobisisobutyronitrile, and dibenzoyl peroxide.
[0059] The mass fraction of the initiator is 0.01 to 10 wt%.
[0060] According to some embodiments of the present invention, the catalyst includes tetramethylethylenediamine, which is a catalyst for free radical polymerization and can accelerate the polymerization reaction.
[0061] In step S3, when the functional component is sodium bicarbonate, the ratio of sodium bicarbonate to the first intermediate product is (2-3) g: (50-70) mL.
[0062] In step S3, when there are functional components, the mass ratio of the functional component sodium bicarbonate, the hydrophilicity regulator methacrylamide, the initiator potassium persulfate and the catalyst tetramethylethylenediamine is 1-3:0.005-0.01:1-2:0.002-0.005.
[0063] In addition to the deacidification property, a chelating agent can be added to the system of the present invention to replace the deacidification component to remove deposited salt and rust from the surface of the protected material. Common desalting and rust removal components include catechol, 1,10-phenanthroline, ethylenediaminetetraacetic acid (EDTA) and its potassium salt and sodium salt, etc. In addition, drugs can also be doped into the self-dissolving hydrogel system of the present invention to achieve the purpose of sustained release.
[0064] According to some embodiments of the present invention, the ultraviolet lamp irradiation time is 1 hour to 3 hours.
[0065] According to some embodiments of the present invention, the ultraviolet lamp irradiation time is 2h to 3h.
[0066] According to some embodiments of the present invention, the method further comprises soaking the product of step S3 in a calcium sulfate solution.
[0067] Calcium sulfate is mainly used to improve the stretchability of the mechanical properties of hydrogels. Calcium ions in the calcium sulfate solution will diffuse into the polymer network and form ionic crosslinks with the carboxylic acid groups of sodium alginate, providing the hydrogel with a three-dimensional network other than covalent crosslinks. The three-dimensional network composed of covalent bonds has a large bond energy and a fixed bond angle, so although it can improve the strength of the hydrogel, it is prone to breakage. The ionic crosslinking based on ionic interactions does not have a fixed bond angle and has a weak bond energy. It can act as a sacrificial bond to inhibit the breakage of the covalent network, thereby improving the stretchability of the hydrogel. In addition to mechanical properties, the ionic crosslinking effect of calcium ions will also affect the rheological properties of the hydrogel, increase the crosslinking degree of the three-dimensional network of the polymer, and thus prolong the time required for the self-dissolving hydrogel to solubilize.
[0068] Soaking in calcium sulfate solution can further regulate the self-dissolution time of the hydrogel.
[0069] The temperature of the calcium sulfate solution for soaking is 25-40°C, preferably 35-40°C.
[0070] The soaking time in the calcium sulfate solution is 4-8 hours, preferably 6-7 hours.
[0071] After soaking, take it out and use nitrogen to blow away excess moisture on the surface.
[0072] The third aspect of the present invention provides the use of the self-dissolving antibacterial hydrogel of the first aspect in food, building materials and archaeological materials.
[0073] The present invention provides a technical solution for the application of self-dissolving antibacterial hydrogel in food, building materials and archaeological materials, which has at least the following beneficial effects:
[0074] In food applications, it can be used as a lining or covering for food packaging to provide moisture retention and preservation effects, extending the shelf life of food. The antibacterial properties can protect food from bacterial contamination and improve food safety.
[0075] In building materials, hydrogels can be used as coatings or concrete additives to improve the waterproofness and durability of building materials. The antibacterial properties can effectively prevent mold growth on the surface of building materials and improve the quality of indoor environment.
[0076] In the application of archaeological materials, it can be used as a coating to protect archaeological relics, prevent pollution and aging on the surface of the relics, and extend their preservation time. It can provide protection and restoration functions without destroying the relics themselves, and maintain the original state and value of the relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 Schematic diagram of the mechanism of gel solization.
[0078] Figure 2 It is the antibacterial test result of the gel of comparative example 1.
[0079] Figure 3 The following are the results of the antibacterial test of the gel of Example 1.
[0080] Figure 4 The following are the results of the antibacterial test of the gel of Example 2.
[0081] Figure 5 This is the product state of the hydrogels of Example 1, Example 2 and Comparative Example 2 after standing for 7 days.
[0082] Figure 6 This is the rheometer test result when the gel of Example 1 is prepared.
[0083] Figure 7 This is the rheometer test result of the gel of Example 1 after three days.
[0084] Figure 8 It is the Fourier infrared spectrum test result of the gel of Example 1, 2 and Comparative Example 1. DETAILED DESCRIPTION
[0085] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0086] In a first aspect, in some embodiments of the present invention, a self-dissolving antibacterial hydrogel is provided, wherein the self-dissolving antibacterial hydrogel comprises an interpenetrating network structure formed by a first polymer and a second polymer, wherein a solvation inducer is distributed in the interpenetrating network structure, wherein the first polymer comprises polyacrylamide, the second polymer comprises at least one of sodium alginate, polyacrylic acid and polymethacrylic acid, and the solvation inducer comprises silver nanoparticles.
[0087] It can be understood that the present invention utilizes a solubilization inducing agent to regulate the interaction of the polymer interpenetrating network in the hydrogel, without the need to introduce a catalyst or enzyme, that is, without the need for a chemical reaction, to achieve the disintegration of the cross-linked polymer network in the hydrogel and the transformation of the hydrogel from a gel to a sol at room temperature. Figure 1In addition to being used for wound dressings, this hydrogel is also of great significance for the rescue moisturizing and reinforcement of fragile materials, as well as for promoting the application of hydrogels in the fields of food, construction, archaeology, etc.
[0088] It should be noted that when the solubilization inducer is silver nanoparticles, the hydrogel based on the regulation of rheological properties by silver nanoparticles has good antibacterial properties, which can not only provide antibacterial protection as a dressing, but also solve the problem of bacterial growth during the preservation of the hydrogel itself.
[0089] It can also be understood that the self-dissolving hydrogel of the present invention can be used as a base material for drug sustained release, chelation, and deacidification components. After being solvated, it is attached to the sample surface in the form of a coating. The problem of residual base material can be solved by simple cleaning, and the release of functional components such as drug sustained release, chelation, and deacidification can also be regulated during the solvation process.
[0090] In the self-dissolving hydrogel of the present invention, the first polymer provides a covalent cross-linking network for the hydrogel. The first polymer, such as sodium alginate, is a commonly used polymer containing carboxylic acid groups and is used to provide ionic cross-linking for the hydrogel.
[0091] The invention improves the preparation of nano silver, the nano silver is formed in a mixed system of sodium alginate and acrylamide, the heating link is reduced, the energy is saved, and the nano silver is evenly distributed inside the hydrogel.
[0092] The invention mixes nano silver with hydrogel to prepare nano silver antibacterial self-dissolving hydrogel, changes the cross-linking structure of the macromolecules inside the hydrogel, not only enhances the mechanical properties of the hydrogel, but also enables the hydrogel to have the self-dissolving property of solubilization over time.
[0093] The preparation method involved in the invention is simple, has strong controllability, can realize mass production, and has high practical value.
[0094] In combination with the first aspect, in some embodiments of the present invention, the content of silver nanoparticles in the hydrogel is 0.001 g / L to 10.00 g / L.
[0095] In combination with the first aspect, in some embodiments of the present invention, the content of silver nanoparticles in the hydrogel is any value among 0.01 g / L, 0.02 g / L, 0.03 g / L, 0.04 g / L, 0.05 g / L, 0.06 g / L, 0.07 g / L, 0.08 g / L, 0.09 g / L, 0.10 g / L, or a range formed by any two of them.
[0096] In combination with the first aspect, in some embodiments of the present invention, the content of silver nanoparticles in the hydrogel is any value among 0.1 g / L, 0.2 g / L, 0.3 g / L, 0.4 g / L, 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L, 1.0 g / L or a range formed by any two of them.
[0097] In combination with the first aspect, in some embodiments of the present invention, the content of silver nanoparticles in the hydrogel is any value among 1g / L, 2g / L, 3g / L, 4g / L, 5 / L, 6g / L, 7g / L, 8g / L, 9g / L, 10g / L or a range formed by any two of them.
[0098] In combination with the first aspect, in some embodiments of the present invention, a functional component is further distributed in the self-dissolving antibacterial hydrogel, and the functional component includes at least one of a deacidifying agent and a chelating agent.
[0099] In combination with the first aspect, in some embodiments of the present invention, the deacidification agent includes at least one of sodium bicarbonate, sodium hydroxide, calcium carbonate, calcium bicarbonate, magnesium oxide, sodium bicarbonate, sodium carbonate, potassium carbonate, potassium bicarbonate and calcium oxide. These inorganic salts or oxides of corresponding metals can be used as alternative deacidification components to reduce the surface acidity of the protected material.
[0100] In combination with the first aspect, in some embodiments of the present invention, the chelating agent includes catechol, 1,10-phenanthroline, ethylenediaminetetraacetic acid (EDTA) and its potassium salt and sodium salt. The chelating agent can replace the deacidification component to remove deposited salt and rust from the surface of the protected material.
[0101] In combination with the first aspect, in some embodiments of the present invention, the functional component further includes a drug with a therapeutic effect, and the purpose of sustained release can be achieved by doping the drug into the self-dissolving hydrogel system of the present invention.
[0102] In a second aspect, in some embodiments of the present invention, there is provided a method for preparing the self-dissolving antibacterial hydrogel of the first aspect of the present invention, comprising the following steps:
[0103] S1: mixing the first polymer monomer, the second polymer and the cross-linking agent and evacuating the mixture to obtain a precursor solution;
[0104] S2: adding a silver nitrate precursor and a reducing agent to the precursor solution, stirring for the first time in the dark, to obtain a first intermediate product;
[0105] S3: adding a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark for a second time, and then irradiating with ultraviolet light to obtain a self-dissolving antibacterial hydrogel; or, step S3 includes: adding a functional component, a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark, and then irradiating with ultraviolet light to obtain a self-dissolving antibacterial hydrogel.
[0106] It can be understood that the preparation method of the present invention does not require expensive equipment and complex process control, the reaction conditions are not harsh, the raw materials are easily available, the production cost is low, and it is easy to industrialize production.
[0107] The preparation method of the present invention uses ultraviolet light irradiation during the preparation process, does not require high temperature conditions, can complete the preparation of hydrogel at room temperature, and avoids the possibility of heat-sensitive substances being denatured or destroyed by heat. The use of a precursor solution can obtain a preliminary intermediate product through simple mixing, vacuum extraction and other steps, so that the preparation process is relatively efficient and the manufacturing cost is reduced. In the stage of the formation of the second intermediate product, by adding functional components, hydrophilicity regulators, initiators and catalysts, the release of functional components such as drug sustained release, chelation, deacidification in the hydrogel can be accurately regulated, thereby increasing the application flexibility of the hydrogel. Adding a solubilization inducer, such as silver nanoparticles, can effectively improve the antibacterial properties of the hydrogel.
[0108] Since self-dissolving antibacterial hydrogel not only has antibacterial properties, it can also be used in construction, food, archaeology and other fields, expanding its market potential and practical application scenarios.
[0109] The preparation method of the present invention does not require the use of a large amount of organic solvents or high-energy consumption equipment during the preparation process, is relatively environmentally friendly, and meets the sustainable development requirements of modern manufacturing.
[0110] In combination with the second aspect, in some embodiments of the present invention, the mass ratio of the first polymer monomer to the second polymer is 1:3-10.
[0111] In conjunction with the second aspect, in some embodiments of the present invention, the first polymer monomer includes acrylamide.
[0112] In combination with the second aspect, in some embodiments of the present invention, the second polymer includes sodium alginate, which is a commonly used polymer containing carboxylic acid groups and is used to provide ionic crosslinking for hydrogels. It can also be replaced by polyacrylic acid or polymethacrylic acid, and its content in the polymerization reaction precursor is 0.1wt% to 10wt%.
[0113] In combination with the second aspect, in some embodiments of the present invention, the crosslinking agent includes at least one of N,N'-methylenebisacrylamide, divinylbenzene, N,N'-(1,2-dihydroxyethylene)diacrylamide, ethylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate and triethylene glycol dimethacrylate.
[0114] In combination with the second aspect, in some embodiments of the present invention, the added amount of the cross-linking agent is 0.01 wt % to 10.0 wt % of the first polymer monomer.
[0115] In conjunction with the second aspect, in some embodiments of the present invention, the solvation inducing agent precursor includes silver nitrate.
[0116] The ratio of silver nitrate to precursor solution is (0.001-0.003) g: (50-70) mL.
[0117] In combination with the second aspect, in some embodiments of the present invention, the reducing agent includes citrate (such as sodium citrate), glucose, formaldehyde, tartrate, and nanocellulose, which reacts with silver nitrate to reduce monovalent silver into elemental silver and form silver nanoparticles through coordination.
[0118] In combination with the second aspect, in some embodiments of the present invention, the mass ratio of the solvation inducing agent precursor to the reducing agent is 1:20-270.
[0119] In step S1, the first polymer monomer, the second polymer and the cross-linking agent are mixed and then vacuumed. The mixture may be stirred at 25-35° C. for 5-9 hours, and then vacuumed at 0.01 MPa for 3-5 hours.
[0120] In step S1, the first polymer monomer, the second polymer and the cross-linking agent are mixed and then vacuumed, and stirred at 25-28° C. for 6-8 hours.
[0121] In step S2, the second polymer sodium alginate is dissolved during the stirring process.
[0122] When the second polymer is sodium alginate, the ratio of sodium alginate to water is (1-2) g: (50-70) mL.
[0123] Water is deionized water and ultrapure water.
[0124] The sodium alginate is high viscosity sodium alginate, more preferably liquid phase sodium alginate.
[0125] In combination with the second aspect, in some embodiments of the present invention, the first light-proof stirring time is 20 min to 30 min.
[0126] In combination with the second aspect, in some embodiments of the present invention, the first light-proof stirring time is 20 min to 25 min.
[0127] The first intermediate product is a solution containing monomers and silver nanoparticles, in which silver nitrate is converted into silver nanoparticles by sodium citrate on the basis of a precursor solution. The solution contains monomers and crosslinking agents containing carbon-carbon double bonds required for polymerization and can form a hydrogel by free radical polymerization.
[0128] In combination with the second aspect, in some embodiments of the present invention, the time of the second light-proof stirring is 20s to 80s.
[0129] In combination with the second aspect, in some embodiments of the present invention, the second light-shielded stirring time is 20s to 25s.
[0130] In conjunction with the second aspect, in some embodiments of the present invention, the functional component includes sodium bicarbonate, which can reduce the acidity of the surface of the protected material when the hydrogel is used as a dressing, and play a role in neutralizing the acidity. Other drugs can also be used instead for other applications, such as chelating agents, weak acids, etc. can be used to remove stubborn inorganic salt deposits.
[0131] In conjunction with the second aspect, in some embodiments of the present invention, the hydrophilicity regulator includes methacrylamide, which is a monomer used to replace acrylamide to change the hydrophilicity of the polymer network, thereby controlling the volume change of the hydrogel after reaching swelling equilibrium.
[0132] In combination with the second aspect, in some embodiments of the present invention, the initiator includes potassium persulfate, which is used to initiate free radical polymerization, and may also be replaced by other initiators such as azobisisobutyronitrile, dibenzoyl peroxide, etc.
[0133] In combination with the second aspect, in some embodiments of the present invention, the catalyst includes tetramethylethylenediamine, which is a catalyst for free radical polymerization and can accelerate the polymerization reaction.
[0134] In step S3, when the functional component is sodium bicarbonate, the ratio of sodium bicarbonate to the first intermediate product is (2-3) g: (50-70) mL.
[0135] In step S3, when there are functional components, the mass ratio of the functional component sodium bicarbonate, the hydrophilicity regulator methacrylamide, the initiator potassium persulfate and the catalyst tetramethylethylenediamine is 1-3:0.005-0.01:1-2:0.002-0.005.
[0136] In combination with the second aspect, in some embodiments of the present invention, the ultraviolet light irradiation time is 1 hour to 3 hours.
[0137] In combination with the second aspect, in some embodiments of the present invention, the ultraviolet light irradiation time is 2h to 3h.
[0138] In combination with the second aspect, in some embodiments of the present invention, the method includes soaking the product of step S3 with calcium sulfate.
[0139] Soaking in calcium sulfate solution can further regulate the self-dissolution time of the hydrogel.
[0140] It should be noted that calcium sulfate itself is slightly soluble in water, and only a very small amount of calcium ions is needed to achieve the performance regulation of sodium alginate hydrogel. A high concentration of calcium ions will have a poor effect.
[0141] The temperature of the calcium sulfate solution for soaking is 25-40°C, preferably 35-40°C.
[0142] The soaking time in the calcium sulfate solution is 4-8 hours, preferably 6-7 hours.
[0143] After soaking, take it out and use nitrogen to blow dry the excess water on the surface of the hydrogel.
[0144] In conjunction with the second aspect, in some embodiments of the present invention, the preparation method may be:
[0145] (1) uniformly mixing sodium alginate and acrylamide in water in a mass ratio of (1-2):(6-10), stirring at 25-35° C. for 5-9 hours, and then vacuuming at 0.01 MPa for 3-5 hours to obtain a precursor solution for a polymerization reaction;
[0146] (2) slowly adding silver nitrate and sodium citrate in a mass ratio of (1-3):(60-270) to the precursor solution and stirring in the dark for 20-30 minutes to obtain a first intermediate product;
[0147] (3) adding sodium bicarbonate, methacrylamide, potassium persulfate and tetramethylethylenediamine in a mass ratio of (1-3):(0.005-0.01):(1-2):(0.002-0.005) to the intermediate product 1, stirring for 20-80 seconds in a light-proof environment, and then irradiating with an ultraviolet lamp with a power of 8W and a wavelength of 254nm for 1-3 hours to obtain a self-dissolving antibacterial hydrogel;
[0148] (4) The self-dissolving antibacterial hydrogel was immersed in a saturated solution of calcium sulfate at 25-40° C. for 4-8 hours, and then taken out and air-dried with nitrogen for 1 minute.
[0149] In step (1):
[0150] The ratio of sodium alginate to water is (1-2) g: (50-70) mL.
[0151] The water is deionized water or ultrapure water, and ultrapure water is more preferred.
[0152] The sodium alginate is high viscosity sodium alginate, more preferably liquid phase sodium alginate.
[0153] The stirring temperature is 25-35°C; more preferably 25-28°C.
[0154] The stirring time is 5-9h, more preferably 6-8h.
[0155] The stirring process is the dissolution process of sodium alginate.
[0156] In step (2):
[0157] The ratio of silver nitrate to precursor solution is (0.001-0.003) g: (50-70) mL.
[0158] The light-proof stirring time is 20-30 min, more preferably 20-25 min.
[0159] The stirring process is the process of reducing silver nitrate to nano-silver and dispersing it.
[0160] In step (3):
[0161] The ratio of sodium bicarbonate to intermediate product 1 is (2-3) g: (50-70) mL.
[0162] The stirring time is 20-80 s, more preferably 20-25 s.
[0163] The stirring process is the polymer cross-linking process.
[0164] The irradiation time is 1-3 h, more preferably 2-3 h.
[0165] In step (4):
[0166] The soaking temperature is 25-40°C, more preferably 35-40°C.
[0167] The soaking time is 4-8 hours, more preferably 6-7 hours.
[0168] The soaking process is the ion exchange process.
[0169] In a third aspect, in some embodiments of the present invention, there is provided use of the self-dissolving antibacterial hydrogel according to the first aspect of the present invention in food, building materials and archaeological materials.
[0170] It can be understood that in food applications, it can be used as a lining or covering for food packaging to provide moisture retention and preservation effects, extending the shelf life of food. The antimicrobial properties can protect food from bacterial contamination and improve food safety.
[0171] In addition, in building materials, hydrogels can be used as coatings or concrete additives to improve the waterproofness and durability of building materials. The antibacterial properties can effectively prevent mold growth on the surface of building materials and improve the quality of indoor environment.
[0172] Furthermore, in the application of archaeological materials, it can be used as a coating for the protection of archaeological relics, preventing the surface pollution and aging of the relics and prolonging their preservation time. It can provide protection and restoration functions without destroying the relics themselves, and maintain the original state and value of the relics.
[0173] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0174] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0175] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0176] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0177] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0178] Acrylamide (AR, 99.0%) and sodium citrate (98%) were purchased from Aladdin-Chemicals.
[0179] Potassium persulfate (GR, 99.9%), potassium bicarbonate (AR, 99.5%), and N,N,N′,N′-tetramethylethylenediamine (99%) were purchased from Macklin’s reagent.
[0180] N,N-Methylenebisacrylamide (MBAA, 98%) was purchased from Maya Reagents.
[0181] Silver nitrate (99%) was purchased from Alfa Aesar.
[0182] Sodium alginate (AR, 98%) was purchased from Rowan.
[0183] Example 1
[0184] A self-dissolving antibacterial hydrogel was prepared, and the specific steps were as follows:
[0185] (1) Weigh 1 g of sodium alginate and 18 g of acrylamide into a beaker, add 60 mL of water, stir at 25 °C for 7 h under the action of a magnetic stirrer, and then use a water pump to evacuate at 0.01 MPa for 4 h to obtain a precursor solution.
[0186] (2) Weigh 0.003 g of silver nitrate and slowly add it to the precursor solution. After stirring thoroughly under a magnetic stirrer in the dark, slowly add 0.03 g of sodium citrate and then stir under a magnetic stirrer in the dark for 25 min to obtain an intermediate product.
[0187] (3) Weigh 3 g of sodium bicarbonate, 0.005 g of N,N-methylenebisacrylamide and 1.5 g of potassium persulfate, measure 25 uL of tetramethylethylenediamine, add them to the intermediate product, and then stir for 40 seconds in a dark environment and under the action of a magnetic stirrer. After the mixture is evenly mixed, irradiate it with an ultraviolet lamp with a power of 8 W and a wavelength of 254 nm for 2 hours to obtain a self-dissolving antibacterial hydrogel.
[0188] (4) In order to further regulate the self-dissolution time of the hydrogel, the self-dissolving antibacterial hydrogel was immersed in a saturated solution of calcium sulfate at 30°C for 6 h and then air-dried with nitrogen for 1 min.
[0189] Example 2
[0190] A self-dissolving antibacterial hydrogel was prepared, and the specific steps were as follows:
[0191] (1) Weigh 2 g of sodium alginate and 13 g of acrylamide into a beaker, add 70 mL of water, stir at 25 °C for 7 h under the action of a magnetic stirrer, and then use a water pump to evacuate at 0.01 MPa for 5 h to obtain a precursor solution.
[0192] (2) Weigh 0.005 g of silver nitrate and slowly add it to the precursor solution. After fully stirring under a magnetic stirrer in the dark, slowly add 0.05 g of sodium citrate and then stir under a magnetic stirrer in the dark for 30 min to obtain an intermediate product.
[0193] (3) Weigh 4 g of sodium bicarbonate, 0.007 g of N,N-methylenebisacrylamide and 2 g of potassium persulfate, measure 30 uL of tetramethylethylenediamine, add them to the intermediate product, and then stir for 40 seconds in a dark environment and under the action of a magnetic stirrer. After the mixture is evenly mixed, irradiate it with an ultraviolet lamp with a power of 8 W and a wavelength of 254 nm for 2 hours to obtain a self-dissolving antibacterial hydrogel.
[0194] (4) In order to further regulate the self-dissolution time of the hydrogel, the self-dissolving antibacterial hydrogel was immersed in a saturated solution of calcium sulfate at 30°C for 4-8 h and then air-dried with nitrogen for 1 min.
[0195] Comparative Example 1
[0196] A hydrogel was prepared, and the specific steps were as follows:
[0197] (1) Weigh 1 g of sodium alginate and 18 g of acrylamide into a beaker, add 60 mL of water, stir at 25 °C for 7 h under the action of a magnetic stirrer, and then use a water pump to evacuate at 0.01 MPa for 4 h to obtain a precursor solution.
[0198] (2) Weigh 3 g of sodium bicarbonate, 0.005 g of N,N-methylenebisacrylamide and 1.5 g of potassium persulfate, measure 25 uL of tetramethylethylenediamine, add them to the precursor solution, and then stir for 40 seconds in a dark environment and under the action of a magnetic stirrer. After the mixture is evenly mixed, irradiate it with an ultraviolet lamp with a power of 8 W and a wavelength of 254 nm for 2 hours to obtain an intermediate product.
[0199] (3) The intermediate product was immersed in a saturated solution of calcium sulfate at 30°C for 6 h, and then air-dried with nitrogen for 1 min to obtain the final product, calcium ion cross-linked hydrogel.
[0200] Comparative Example 2
[0201] A hydrogel was prepared, and the specific steps were as follows:
[0202] (1) 2 g of sodium alginate and 13 g of acrylamide were added to a beaker, and 70 mL of water was added. The mixture was stirred at 25 °C for 7 h under a magnetic stirrer, and then a water pump was used to evacuate the mixture at 0.01 MPa for 5 h to obtain a precursor solution.
[0203] (2) Weigh 4 g of sodium bicarbonate, 0.007 g of N,N-methylenebisacrylamide and 2 g of potassium persulfate, measure 30 uL of tetramethylethylenediamine, add them to the precursor solution, and then stir for 40 seconds in a dark environment and under the action of a magnetic stirrer. After the mixture is evenly mixed, irradiate it with an ultraviolet lamp with a power of 8 W and a wavelength of 254 nm for 2 hours to obtain an intermediate product.
[0204] (3) The intermediate product was immersed in a saturated solution of calcium sulfate at 30° C. for 4-8 h, and then air-dried with nitrogen for 1 min to obtain the final product, nanosilver antibacterial self-dissolving hydrogel.
[0205] Comparative Example 3
[0206] A hydrogel was prepared, and the specific steps were as follows:
[0207] (1) Weigh 2 g of sodium alginate and 13 g of acrylamide into a beaker, add 70 mL of water, stir at 25 °C for 7 h under the action of a magnetic stirrer, and then use a water pump to evacuate at 0.01 MPa for 5 h to obtain a precursor solution.
[0208] (2) Weigh 0.005 g of silver nitrate and slowly add it to the precursor solution. After being fully stirred under a magnetic stirrer while protecting from light, an intermediate product 1 is obtained.
[0209] (3) Weigh 4 g of sodium bicarbonate, 0.007 g of N,N-methylenebisacrylamide and 2 g of potassium persulfate, measure 30 uL of tetramethylethylenediamine, add them to the intermediate product 1, and then stir for 40 seconds in a dark environment and under the action of a magnetic stirrer. After the mixture is evenly mixed, irradiate it with an ultraviolet lamp with a power of 8 W and a wavelength of 254 nm for 2 hours to obtain a hydrogel.
[0210] (4) The hydrogel was immersed in a saturated solution of calcium sulfate at 30°C for 4-8 hours, and then air-dried with nitrogen for 1 minute.
[0211] Antibacterial test
[0212] The hydrogels of Comparative Example 1 and Example 1 and Example 2 were used in antibacterial experiments to verify that the self-dissolving hydrogel prepared by the present invention has antibacterial effect.
[0213] Configuration 10 6 The E. coli solution with a concentration of CFU / mL was inoculated in a common beef peptone culture medium. The hydrogel-filled antibacterial rings were taken from Comparative Example 1 and Example 1 and Example 2 and placed on the culture medium. After culturing at 37°C for 24 hours, the antibacterial ring test results were obtained. The above experimental results are shown in Figures 2 to 4 shown.
[0214] Figure 2 It is the antibacterial test result of the gel of comparative example 1.
[0215] Figure 3 The following are the results of the antibacterial test of the gel of Example 1.
[0216] Figure 4 The following are the results of the antibacterial test of the gel of Example 2.
[0217] The antibacterial ring in Comparative Example 1 is almost invisible, and the bacteria grow all over the culture medium, indicating that the hydrogel sample in Comparative Example 1 has no antibacterial properties, while obvious antibacterial rings appear in Examples 1 and 2, and the diameters of the antibacterial rings in Examples 1 and 2 are slightly different.
[0218] Depend on Figures 2 to 4 It can be seen that both Example 1 and Example 2, in which nanosilver particles are added to the hydrogel, achieve good antibacterial effects, while Comparative Example 1, in which nanosilver particles are not added, has no antibacterial effect.
[0219] The hydrogels obtained in Example 1, Example 2 and Comparative Example 2 were placed in a room at 30° C. and away from light. After standing for 7 days, the final product was obtained as shown in Figure 5 As shown, it can be seen that the hydrogels of Example 1 and Example 2 both showed self-dissolution, while the comparative example 2 did not show self-dissolution, indicating that the nanosilver particles played a decisive role in the degradation process of the hydrogel.
[0220] Furthermore, the rheological data of Example 1 were tested by a rheometer, with the test conditions being 25°C and an angular frequency of 1-100 rad / s. Figure 6 It can be seen that when Example 1 is just prepared, the storage modulus is significantly higher than the loss modulus, and the storage modulus curve has no intersection with the loss modulus curve, indicating that it is in a stable gel state at different angular frequencies. Figure 7 It can be seen that after Example 1 is placed for 3 days, the storage modulus and loss modulus will have an intersection, which is the gel point. At the gel point, the shear stress of the sample begins to increase significantly, indicating that the sample is in a sol state under low angular frequency conditions, and gradually gels and becomes a gel state as the angular frequency increases. The before and after comparison shows that Example 1 changes from a gel state when it is just prepared to a sol with a certain fluidity after 3 days during the placement process.
[0221] The chemical structures of the hydrogels of Example 1, Example 2 and Comparative Example 1 were characterized using a Fourier transform infrared absorption spectrometer. The hydrogel samples were dried at 60°C for 12 hours to form a dry polymer film for Fourier transform infrared absorption spectroscopy analysis. -1 Spectra were obtained within the range.
[0222] like Figure 8 As shown, at 3400-3200cm -1 The absorption peak in the range 1614cm corresponds to the stretching vibration of the hydroxyl group of sodium alginate. -1 and 1398cm -1 The absorption peaks at 1652 cm-1 correspond to the asymmetric stretching vibration and symmetric stretching vibration of the O=CO group. -1 and 1604cm -1Asymmetric and symmetric vibration peaks of the C=O group in polyacrylamide can be observed at 3355cm -1 and 3192cm -1 The absorption peaks obtained at are caused by the stretching vibrations of the hydroxyl group and the amino group, respectively.
[0223] The self-dissolving hydrogel of the present invention is composed of an antibacterial hydrogel formed by sodium alginate and polyacrylamide and a small amount of silver nanoparticles, and has multiple social, economic and technical advantages. Socially, this hydrogel can effectively inhibit bacterial growth and help reduce bacterial and fungal erosion of protected samples. Economically, sodium alginate and polyacrylamide are low-cost and widely available raw materials, the preparation process is relatively simple, and the production cost is relatively low, which helps to reduce medical care costs and improve the efficiency of medical resource utilization. The method for preparing silver nanoparticles also has the characteristics of low cost and simple process. Technically, the hydrogel not only has excellent water adsorption capacity, but also has adjustable solubilization characteristics, can flexibly respond to needs under different environmental conditions, and reduce damage to the protected materials, showing broad application potential and market value.
[0224] Finally, it should be noted that the conversion of the gel to sol of the present invention refers to the conversion of the entire material, not limited to the surface of the material. The conversion of the gel solvent in the prior art is mainly caused by the change of ionic crosslinking as the cause of the gel-sol conversion. In addition to ionic crosslinking, the present invention also has the result of the entanglement and coordination of the polymer network.
[0225] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A self-dissolving antibacterial hydrogel, characterized in that: The self-dissolving antibacterial hydrogel comprises an interpenetrating network structure formed by a first polymer and a second polymer, wherein a solubilization inducing agent is distributed in the interpenetrating network structure, wherein the first polymer comprises polyacrylamide, the second polymer comprises at least one of sodium alginate, polyacrylic acid and polymethacrylic acid, and the solubilization inducing agent comprises silver nanoparticles.
2. The self-dissolving antibacterial hydrogel according to claim 1, characterized in that: Functional components are also distributed in the self-dissolving antibacterial hydrogel, and the functional components include at least one of a deacidifying agent and a chelating agent.
3. A method for preparing the self-dissolving antibacterial hydrogel according to claim 1 or 2, characterized in that: The following steps are involved: S1: mixing the first polymer monomer, the second polymer and the cross-linking agent and evacuating the mixture to obtain a precursor solution; S2: adding a solvation inducing agent precursor and a reducing agent to the precursor solution, and stirring for the first time in the dark to obtain a first intermediate product; S3: adding a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark for a second time, and then irradiating with ultraviolet light to obtain the self-dissolving antibacterial hydrogel; or, step S3 includes: adding a functional component, a hydrophilicity regulator, an initiator and a catalyst to the first intermediate product, stirring and reacting in the dark, and then irradiating with ultraviolet light to obtain the self-dissolving antibacterial hydrogel.
4. The method according to claim 3, characterized in that The mass ratio of the first polymer monomer to the second polymer is 1:3 to 10; and / or the cross-linking agent includes at least one of N,N'-methylenebisacrylamide, divinylbenzene, N,N'-(1,2-dihydroxyethylene)diacrylamide, ethylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate and triethylene glycol dimethacrylate; and / or the added amount of the cross-linking agent is 0.01wt% to 10.0wt% of the sum of the mass of the first polymer monomer and the second polymer.
5. The method according to claim 3, characterized in that: The solization inducing agent precursor includes silver nitrate; and / or, the reducing agent includes sodium citrate; and / or, the mass ratio of the solization inducing agent precursor to the reducing agent is 1:20-270.
6. The method according to claim 3, characterized in that The first light-proof stirring time is 20 min to 30 min.
7. The method according to claim 3, characterized in that The second light-proof stirring time is 20s to 80s.
8. The method according to claim 3, characterized in that The power of the ultraviolet lamp is 6W to 10W; and / or the irradiation time of the ultraviolet lamp is 1h to 3h.
9. The method according to claim 3, characterized in that: The method further comprises soaking the product of step S3 with calcium sulfate.
10. Use of the self-dissolving antibacterial hydrogel according to claim 1 or 2 in the preparation of food, building materials and archaeological materials.
Citation Information
Patent Citations
Nano-silver antibacterial hydrogel and preparation method thereof
CN102698313A
Preparation method for sodium alginate-acrylamide-based hydrogel
CN103396562A
Preparation method and application of imidazolium salt ionic liquid / polyvinyl alcohol pressure sensing antibacterial hydrogel dressing
CN114887112A
Hydrogel
US20060052478A1