Biodegradable agricultural film and preparation method thereof
By combining modified polyethylene and modified chitosan, biodegradable agricultural films with flame retardant, UV resistance and self-healing properties are produced, which solves the problem of non-degradable, easy aging and combustion of polyethylene agricultural films, and realizes the Improvement of environmental protection and safety.
Patent Information
- Application Number
- CN202411140462.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polyethylene agricultural films are non-degradable in nature and are prone to aging and burning, resulting in environmental pollution and safety hazards, and have limited service life.
The modified polyethylene and modified chitosan were used to produce biodegradable agricultural films by mixing extrusion and granulation films. The modified polyethylene was modified by grafting 4-vinylbenzene boric acid and allyl phosphate diethyl phosphate. Chitosan reacts 3,4-dihydroxyaniline and oxalyl chloride monomethyl ester to form a material with flame retardant, UV resistance and self-healing properties.
The flame retardant, ultraviolet aging and self-repair properties of biodegradable agricultural films are achieved, reducing environmental pollution and use costs, and improving safety.
Smart Images

Figure BDA0005000637740000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a biodegradable agricultural film and a preparation method thereof. Background Art
[0002] Agricultural film, also known as ground film, is often used to cover farmland to maintain soil moisture and temperature to meet the necessary conditions for crop growth, improve crop yield and quality, and is widely used in agricultural production.
[0003] Polyethylene is a polymer material widely used in the production of agricultural films. It is favored for its high cost-effectiveness, good light transmittance and thermal insulation. However, since polyethylene is not degradable in nature in a short period of time, it is very easy to pollute the ecological environment. In addition, polyethylene agricultural films are used outdoors for a long time and are prone to aging under ultraviolet rays, resulting in a limited service life of the agricultural films. Polyethylene is also a highly flammable material and is easily burned when exposed to open flames in a dry environment, posing a safety hazard. Therefore, preparing a biodegradable, UV-resistant, flame-retardant polyethylene agricultural film can reduce environmental pollution, reduce the cost of using agricultural films, and increase safety. Summary of the invention
[0004] The purpose of the present invention is to provide a biodegradable agricultural film and a preparation method thereof to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A biodegradable agricultural film is prepared by mixing, extruding, granulating and pressing modified polyethylene and modified chitosan.
[0007] As an optimization, the modified polyethylene is prepared by grafting 4-vinylbenzeneboric acid and diethyl allyl phosphate onto polyethylene.
[0008] As an optimization, the modified chitosan is prepared by first reacting 3,4-dihydroxyaniline with methyl oxalyl chloride to obtain oxalylanilide monomer, and then reacting the monomer with chitosan.
[0009] A method for preparing a biodegradable agricultural film comprises the following preparation steps:
[0010] (1) 3,4-dihydroxyaniline, triethylamine and dichloromethane are mixed in a mass ratio of 1:(1.1-1.2):(10-12) to obtain a mixed solution A, 1.15-1.2 times the mass of 3,4-dihydroxyaniline monomethyl chloride and dichloromethane are mixed in a mass ratio of 1:(10-12) to obtain a mixed solution B, the mixed solution B is added dropwise to the mixed solution A at a rate of 0.1 mL / min at 0-4° C., the temperature is raised to room temperature after the addition is completed, the mixture is stirred for 3-4 hours, pure water in an amount of 20-25 times the mass of 3,4-dihydroxyaniline is added, and ethyl acetate in an amount of 20-25 times the mass of 3,4-dihydroxyaniline is added for extraction, the lower organic phase is removed and dried using anhydrous magnesium sulfate, the filtrate is filtered and the ethyl acetate and dichloromethane are removed by vacuum rotary evaporation to obtain an oxalylanilide monomer;
[0011] (2) Add oxalic acid anilide monomer, chitosan and N,N-dimethylformamide in a mass ratio of 1: (1.1-1.2):
[0012] (10-12) The mixture was mixed evenly, heated to 110 °C under a nitrogen atmosphere, stirred for 10-12 h, cooled to room temperature, 3-4 times the mass of N,N-dimethylformamide was added with acetone for precipitation, filtered, and dried at 40 °C for 10-12 h to obtain modified chitosan;
[0013] (3) Under nitrogen protection, at 95° C., polyethylene and dichloromethane were mixed at a mass ratio of 1:(20-25) for 10-20 min, 4-vinylbenzeneboric acid (0.3-0.5 times the mass of polyethylene), diethyl allyl phosphate (0.2-0.3 times the mass of polyethylene), and benzoyl peroxide (0.1 times the mass of polyethylene) were added, and the reaction was continued for 3-4 h. Acetone (3-4 times the volume of dichloromethane) was added for precipitation, and the mixture was filtered and washed with acetone for 3-4 times, and dried at 60° C. for 5-6 h to obtain modified polyethylene;
[0014] (4) The modified polyethylene and the modified chitosan are uniformly mixed in a mass ratio of 1:(0.1-0.15), added to a banbury mixer and kneaded for 5-10 minutes to obtain a masterbatch, the masterbatch is put into a twin-screw extruder for extrusion, and then granulated, and pressed into a film using a flat plate vulcanizer.
[0015] As an optimization, the internal mixing temperature of step (4) is 150°C; the temperature of the twin-screw extruder is 160°C, and the rotation speed is 500rpm / min; the film pressing temperature of the flat plate vulcanizer is 140°C, the pressure is 10MPa, and the time is 7min.
[0016] As an optimization, the deacetylation degree of the chitosan in step (2) is 90.6%.
[0017] As an optimization, the model of the polyethylene in step (3) is DFDA-7042.
[0018] As an optimization, the modified chitosan in step (2) contains an oxalylanilide group, which has ultraviolet absorption properties and can convert the absorbed ultraviolet energy into heat energy. The conversion diagram is as follows:
[0019]
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] When preparing the biodegradable agricultural film, the present invention comprises the following steps: firstly grafting polyethylene with 4-vinylbenzeneboronic acid and diethyl allyl phosphate to obtain modified polyethylene; then reacting 3,4-dihydroxyaniline and methyl oxalyl chloride to obtain oxalylanilide monomer, and then reacting the monomer with chitosan to obtain modified chitosan; finally, mixing the modified polyethylene and the modified chitosan, extruding, granulating and pressing the mixture to obtain the modified agricultural film.
[0022] Firstly, polyethylene was grafted with 4-vinylbenzeneboric acid and diethyl allyl phosphate by solution polymerization to obtain modified polyethylene, and boric acid and phosphate structures with flame retardant properties were introduced into the polyethylene side chain to give the polyethylene agricultural film good flame retardant properties.
[0023] Then, 3,4-dihydroxyaniline and monomethyl oxalyl chloride are reacted with amino groups and acyl chlorides to obtain oxalylanilide monomers, which are then reacted with chitosan to obtain modified chitosan, so that the chitosan is connected with the oxalylanilide structure. When exposed to ultraviolet rays, the oxalylanilide structure can absorb ultraviolet rays and convert the ultraviolet energy into heat energy for release, thereby achieving the effect of anti-ultraviolet rays and giving the material anti-ultraviolet aging properties. Chitosan, as a natural polysaccharide, has good biodegradability. Mixing chitosan with polyethylene can give polyethylene good biodegradability.
[0024] Finally, the modified polyethylene and modified chitosan are mixed, extruded, granulated and filmed to produce biodegradable agricultural film. The boric acid groups on the modified chitosan and the dihydroxyphenyl groups on the modified polyethylene can form a dynamically reversible borate ester structure, which can not only serve as cross-linking points to increase the bonding between chitosan and modified polyethylene, but also give the polyethylene agricultural film certain self-healing properties. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The model of polyethylene used in the following examples and comparative examples is DFDA-7042; the deacetylation degree of chitosan used is 90.6%.
[0027] Example 1
[0028] A method for preparing a biodegradable agricultural film, the method comprising the following steps:
[0029] (1) 3,4-dihydroxyaniline, triethylamine and dichloromethane are mixed in a mass ratio of 1:1.1:10 to obtain a mixed solution A, 1.15 times the mass of 3,4-dihydroxyaniline monomethyl chloride and dichloromethane are mixed in a mass ratio of 1:10 to obtain a mixed solution B, and the mixed solution B is added dropwise to the mixed solution A at a rate of 0.1 mL / min at 4° C. After the addition is completed, the mixture is heated to room temperature and stirred for 4 hours, and pure water in an amount of 20 times the mass of 3,4-dihydroxyaniline is added, and then ethyl acetate in an amount of 20 times the mass of 3,4-dihydroxyaniline is added for extraction, the lower organic phase is removed and dried using anhydrous magnesium sulfate, the filtrate is filtered and the ethyl acetate and dichloromethane are removed by vacuum rotary evaporation to obtain an oxalylaniline monomer;
[0030] (2) mixing oxalylanilide monomer, chitosan and N,N-dimethylformamide in a mass ratio of 1:1.1:10, heating to 110°C under a nitrogen atmosphere, stirring for 12 h, cooling to room temperature, adding acetone 3 times the mass of N,N-dimethylformamide for precipitation, filtering and drying at 40°C for 12 h to obtain modified chitosan;
[0031] (3) Under nitrogen protection, polyethylene and dichloromethane were mixed at a mass ratio of 1:20 for 20 min at 95 °C, 4-vinylbenzeneboric acid (0.3 times the mass of polyethylene), diethyl allyl phosphate (0.2 times the mass of polyethylene), and benzoyl peroxide (0.1 times the mass of polyethylene) were added, and the reaction was continued for 4 h. Acetone (3 times the volume of dichloromethane) was added for precipitation, and the mixture was filtered and washed with acetone for 4 times, and dried at 60 °C for 6 h to obtain modified polyethylene.
[0032] (4) The modified polyethylene and the modified chitosan were mixed uniformly in a mass ratio of 1:0.1, added to a banbury mixer and kneaded for 10 min to obtain a masterbatch, which was put into a twin-screw extruder for extrusion, and then granulated and pressed into a film using a flat plate vulcanizer, wherein the kneading temperature in the banbury mixer was 150°C; the temperature of the twin-screw extruder was 160°C, the rotation speed was 500 rpm / min; the film pressing temperature of the flat plate vulcanizer was 140°C, the pressure was 10 MPa, and the time was 7 min.
[0033] Example 2
[0034] A method for preparing a biodegradable agricultural film, the method comprising the following steps:
[0035] (1) 3,4-dihydroxyaniline, triethylamine and dichloromethane are mixed in a mass ratio of 1:1.15:11 to obtain a mixed solution A, 1.17 times the mass of 3,4-dihydroxyaniline monomethyl chloride and dichloromethane are mixed in a mass ratio of 1:11 to obtain a mixed solution B, and the mixed solution B is added dropwise to the mixed solution A at a rate of 0.1 mL / min at 2° C. After the addition is completed, the mixture is heated to room temperature and stirred for 3.5 hours, pure water is added in an amount of 22 times the mass of 3,4-dihydroxyaniline, and ethyl acetate is added in an amount of 22 times the mass of 3,4-dihydroxyaniline to extract, the lower organic phase is removed and dried using anhydrous magnesium sulfate, the filtrate is filtered and the ethyl acetate and dichloromethane are removed by vacuum rotary evaporation to obtain an oxalylanilide monomer;
[0036] (2) mixing oxalylanilide monomer, chitosan and N,N-dimethylformamide in a mass ratio of 1:1.15:11, heating to 110°C under a nitrogen atmosphere, stirring for 11 hours, cooling to room temperature, adding acetone 3.5 times the mass of N,N-dimethylformamide for precipitation, filtering and drying at 40°C for 11 hours to obtain modified chitosan;
[0037] (3) Under nitrogen protection, polyethylene and dichloromethane were mixed at a mass ratio of 1:22 for 15 min at 95 °C, 4-vinylbenzeneboric acid (0.4 times the mass of polyethylene), diethyl allyl phosphate (0.25 times the mass of polyethylene), and benzoyl peroxide (0.1 times the mass of polyethylene) were added, and the reaction was continued for 3.5 h. Acetone (3.5 times the volume of dichloromethane) was added for precipitation, and the mixture was filtered and washed with acetone for 3 times, and dried at 60 °C for 5.5 h to obtain modified polyethylene;
[0038] (4) The modified polyethylene and the modified chitosan were mixed uniformly in a mass ratio of 1:0.12, added to a banbury mixer and kneaded for 7 minutes to obtain a masterbatch, which was put into a twin-screw extruder for extrusion, and then granulated and pressed into a film using a flat plate vulcanizer, wherein the kneading temperature in the banbury mixer was 150°C; the temperature of the twin-screw extruder was 160°C, the rotation speed was 500 rpm / min; the film pressing temperature of the flat plate vulcanizer was 140°C, the pressure was 10 MPa, and the time was 7 minutes.
[0039] Example 3
[0040] A method for preparing a biodegradable agricultural film, the method comprising the following steps:
[0041] (1) 3,4-dihydroxyaniline, triethylamine and dichloromethane are mixed in a mass ratio of 1:1.2:12 to obtain a mixed solution A; 1.2 times the mass of 3,4-dihydroxyaniline monomethyl chloride and dichloromethane are mixed in a mass ratio of 1:12 to obtain a mixed solution B; the mixed solution B is added dropwise to the mixed solution A at a rate of 0.1 mL / min at 0° C.; after the addition is completed, the mixture is heated to room temperature and stirred for 3 h; pure water in an amount of 25 times the mass of 3,4-dihydroxyaniline is added; and ethyl acetate in an amount of 25 times the mass of 3,4-dihydroxyaniline is added for extraction; the lower organic phase is removed and dried over anhydrous magnesium sulfate; the filtrate is filtered and the ethyl acetate and dichloromethane are removed by vacuum rotary evaporation to obtain an oxalylaniline monomer;
[0042] (2) mixing oxalylanilide monomer, chitosan and N,N-dimethylformamide in a mass ratio of 1:1.2:12, heating to 110°C under a nitrogen atmosphere, stirring for 10 h, cooling to room temperature, adding acetone 4 times the mass of N,N-dimethylformamide for precipitation, filtering and drying at 40°C for 10 h to obtain modified chitosan;
[0043] (3) Under nitrogen protection, polyethylene and dichloromethane were mixed at a mass ratio of 1:25 for 10 min at 95 °C, 4-vinylbenzeneboric acid (0.5 times the mass of polyethylene), diethyl allyl phosphate (0.3 times the mass of polyethylene), and benzoyl peroxide (0.1 times the mass of polyethylene) were added, and the reaction was continued for 3 h. Acetone (4 times the volume of dichloromethane) was added for precipitation, and the mixture was filtered and washed with acetone for 4 times, and dried at 60 °C for 5 h to obtain modified polyethylene.
[0044] (4) The modified polyethylene and the modified chitosan were mixed uniformly in a mass ratio of 1:0.15, added to a banbury mixer and kneaded for 5 minutes to obtain a masterbatch, which was put into a twin-screw extruder for extrusion, and then granulated and pressed into a film using a flat plate vulcanizer, wherein the kneading temperature in the banbury mixer was 150°C; the temperature of the twin-screw extruder was 160°C, the rotation speed was 500 rpm / min; the film pressing temperature of the flat plate vulcanizer was 140°C, the pressure was 10 MPa, and the time was 7 minutes.
[0045] Comparative Example 1
[0046] The preparation method of the biodegradable agricultural film of Comparative Example 1 differs from that of Example 2 in that it does not contain steps (1) and (2), and step (4) is modified to uniformly mix the modified polyethylene and chitosan in a mass ratio of 1:0.12, add them to a banbury mixer and knead them for 7 minutes to obtain a masterbatch, put the masterbatch into a twin-screw extruder for extrusion, and then granulate them, and use a flat-plate vulcanizer to press them into a film, wherein the kneading temperature in the banbury mixer is 150°C; the temperature of the twin-screw extruder is 160°C, and the rotation speed is 500rpm / min; the film pressing temperature of the flat-plate vulcanizer is 140°C, the pressure is 10MPa, and the time is 7min.
[0047] Comparative Example 2
[0048] The preparation method of the biodegradable agricultural film of Comparative Example 2 differs from that of Example 2 in that it does not contain steps (1) and (2), and step (4) is modified by adding modified polyethylene into a banbury mixer and kneading for 7 minutes to obtain a masterbatch, which is put into a twin-screw extruder for extrusion, and then granulated and pressed into a film using a flat-plate vulcanizer, wherein the kneading temperature in the banbury mixer is 150°C; the temperature of the twin-screw extruder is 160°C, and the rotation speed is 500rpm / min; the film pressing temperature of the flat-plate vulcanizer is 140°C, the pressure is 10MPa, and the time is 7min.
[0049] Comparative Example 3
[0050] The preparation method of the biodegradable agricultural film of Comparative Example 3 differs from that of Example 2 in that step (3) is not included, and step (4) is modified to uniformly mix polyethylene and modified chitosan in a mass ratio of 1:0.12, add them to a banbury mixer and knead them for 7 minutes to obtain a masterbatch, put the masterbatch into a twin-screw extruder for extrusion, and then granulate them, and use a flat-plate vulcanizer to press them into a film, wherein the kneading temperature of the banbury mixer is 150°C; the temperature of the twin-screw extruder is 160°C, and the rotation speed is 500rpm / min; the film pressing temperature of the flat-plate vulcanizer is 140°C, the pressure is 10MPa, and the time is 7min.
[0051] Test Example 1
[0052] Flame retardant performance test
[0053] Test method: According to the standard GB / T 2406-2009, the degradable agricultural films prepared in the examples and comparative examples were prepared into test specimens with a size of 150 mm×20 mm, and the limiting oxygen index test was performed on the specimens. The results are shown in Table 1.
[0054] Table 1
[0055] Limiting oxygen index (%) Limiting oxygen index (%) Example 1 26.6 Comparative Example 1 25.9 Example 2 27.1 Comparative Example 2 26.4 Example 3 26.7 Comparative Example 3 18.9
[0056] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the biodegradable agricultural film prepared by the present invention has good flame retardant properties.
[0057] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 3, indicating that the modified polyethylene prepared by grafting 4-vinylbenzeneboric acid and diethyl allyl phosphate onto polyethylene by solution polymerization introduces boric acid and phosphate structures with flame retardant properties into the polyethylene side chain, giving the polyethylene agricultural film good flame retardant properties.
[0058] Test Example 2
[0059] Test of anti-ultraviolet aging performance
[0060] Test method: The biodegradable agricultural films prepared in the embodiment and the comparative example were subjected to an anti-ultraviolet aging test in an ultraviolet lamp aging test box, the experimental temperature was 60°C, the relative humidity was 65%, the aging time was 168h, the distance between the agricultural film and the light source was 40mm, the ultraviolet lamp power was 30W, and the wavelength was 320nm. The agricultural films before and after aging were tested for tensile strength according to the standard GB / T 1040.3-2006, and the tensile strength change rate A before and after aging was calculated. The tensile strength change rate calculation formula is as follows: A=(A0-A1) / A0×100%, wherein A0 is the tensile strength before aging, and A1 is the tensile strength after aging. The results are shown in Table 2.
[0061] Table 2
[0062] Tensile strength change rate (%) Tensile strength change rate (%) Example 1 7.1 Comparative Example 1 50.4 Example 2 8.6 Comparative Example 2 51.6 Example 3 6.9 Comparative Example 3 8.7
[0063] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the biodegradable agricultural film prepared by the present invention has good resistance to ultraviolet aging.
[0064] By comparison, the change rates of tensile strength of Examples 1 to 3 are smaller than those of Comparative Examples 1 and 2, indicating that 3,4-dihydroxyaniline and methyl oxalyl chloride are reacted through amino groups and acyl chlorides to obtain oxalylanilide monomers, which are then reacted with chitosan to obtain modified chitosan, so that the oxalylanilide structure is grafted onto the chitosan. When exposed to ultraviolet rays, the oxalylanilide structure can absorb ultraviolet rays and convert the ultraviolet energy into heat energy for release, thereby achieving an anti-ultraviolet effect and giving the material anti-ultraviolet aging properties.
[0065] Test Example 3
[0066] Degradation performance test
[0067] Test method: Referring to the standard GB / T 19275-2003, the agricultural films prepared in the embodiments and comparative examples were cut into samples of 1×1 cm, dried at 40°C to constant weight, and the mass was recorded as W0. The samples were wrapped with gauze and buried in the grass, where the average humidity of the grass was 35%, the pH value was 6.7, and the burial depth was 15 cm. The samples were taken out after 60 days, cleaned, dried and weighed, and the mass was recorded as W1. The degradation rate W was calculated by the following formula: W=(W0-W1) / W0×100%. The results are shown in Table 3.
[0068] Table 3
[0069] Degradation rate (%) Degradation rate (%) Example 1 54.7 Comparative Example 1 51.9 Example 2 54.4 Comparative Example 2 10.4 Example 3 53.6 Comparative Example 3 52.4
[0070] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 3, it can be found that the biodegradable agricultural film prepared by the present invention has good biodegradability.
[0071] By comparison, the degradation rates of Examples 1 to 3 are greater than that of Comparative Example 2, indicating that 3,4-dihydroxyaniline and methyl oxalyl chloride are reacted through an amino group and an acyl chloride to obtain an oxalyl anilide monomer, which is then reacted with chitosan to obtain a modified chitosan. Chitosan, as a natural polysaccharide, has good biodegradability. Mixing chitosan with polyethylene can give polyethylene good biodegradability.
[0072] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A biodegradable agricultural film, characterized in that: The biodegradable agricultural film is made by mixing modified polyethylene and modified chitosan, extruding, granulating and pressing films; The modified polyethylene is prepared by grafting 4-vinylbenzeneboric acid and diethyl allyl phosphate onto polyethylene; The modified chitosan is prepared by firstly reacting 3,4-dihydroxyaniline with methyl oxalyl chloride to obtain oxalylanilide monomer, and then reacting the monomer with chitosan.
2. A method for preparing a biodegradable agricultural film, characterized in that: The method comprises the following preparation steps: (1) 3,4-dihydroxyaniline, triethylamine and dichloromethane are mixed in a mass ratio of 1:(1.1-1.2):(10-12) to obtain a mixed solution A, 1.15-1.2 times the mass of 3,4-dihydroxyaniline monomethyl chloride and dichloromethane are mixed in a mass ratio of 1:(10-12) to obtain a mixed solution B, the mixed solution B is added dropwise to the mixed solution A at a rate of 0.1 mL / min at 0-4° C., the temperature is raised to room temperature after the addition is completed, the mixture is stirred for 3-4 hours, pure water in an amount of 20-25 times the mass of 3,4-dihydroxyaniline is added, and ethyl acetate in an amount of 20-25 times the mass of 3,4-dihydroxyaniline is added for extraction, the lower organic phase is removed and dried using anhydrous magnesium sulfate, the filtrate is filtered and the ethyl acetate and dichloromethane are removed by vacuum rotary evaporation to obtain an oxalylanilide monomer; (2) mixing oxalylanilide monomer, chitosan and N,N-dimethylformamide in a mass ratio of 1:(1.1-1.2):(10-12), heating to 110°C under a nitrogen atmosphere, stirring for 10-12 hours, cooling to room temperature, adding acetone 3-4 times the mass of N,N-dimethylformamide for precipitation, filtering and drying at 40°C for 10-12 hours to obtain modified chitosan; (3) Under nitrogen protection, at 95° C., polyethylene and dichloromethane were mixed at a mass ratio of 1:(20-25) for 10-20 min, 4-vinylbenzeneboric acid (0.3-0.5 times the mass of polyethylene), diethyl allyl phosphate (0.2-0.3 times the mass of polyethylene), and benzoyl peroxide (0.1 times the mass of polyethylene) were added, and the reaction was continued for 3-4 h. Acetone (3-4 times the volume of dichloromethane) was added for precipitation, and the mixture was filtered and washed with acetone for 3-4 times, and dried at 60° C. for 5-6 h to obtain modified polyethylene; (4) The modified polyethylene and the modified chitosan are uniformly mixed in a mass ratio of 1:(0.1-0.15), added to a banbury mixer and kneaded for 5-10 minutes to obtain a masterbatch, the masterbatch is put into a twin-screw extruder for extrusion, and then granulated, and pressed into a film using a flat plate vulcanizer.
3. The method for preparing a biodegradable agricultural film according to claim 2, characterized in that: The internal mixer temperature of step (4) is 150° C.; the temperature of the twin-screw extruder is 160° C. and the rotation speed is 500 rpm / min; the film pressing temperature of the flat plate vulcanizer is 140° C., the pressure is 10 MPa, and the time is 7 min.
4. The method for preparing a biodegradable agricultural film according to claim 2, characterized in that: The deacetylation degree of the chitosan in step (2) is 90.6%.
5. The method for preparing a biodegradable agricultural film according to claim 2, characterized in that: The model of the polyethylene in step (3) is DFDA-7042.
Citation Information
Patent Citations
Epoxy resin curing agent capable of improving anti-ultraviolet performance of epoxy resin and preparation method for epoxy resin curing agent
CN106008926A
Preparation method of environmentally-friendly agricultural mulch film
CN109438943A
Room-temperature self-repairing water-plastic film material and preparation method thereof
CN114716708A
Functional polyethylene composite plastic and manufacturing process thereof
CN116444883A