Wear-resistant resin-based composite material and preparation method thereof

By adding modified silicon carbide whiskers and pretreated carbon fibers to resin-based composite materials, and adding silicone oil and flame retardant, the problem of insufficient wear resistance of existing materials is solved, and the wear resistance and flame retardant performance of the materials is significantly improved , extends service life and enhances mechanical properties.

CN118909392AInactive Publication Date: 2024-11-08TAICANG ZHIBAO TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411095476.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The wear resistance of existing resin-based composite materials is insufficient, resulting in short service life and easy wear, affecting their application performance under complex working conditions.

Method used

By adding modified silicon carbide whiskers and pretreated carbon fibers to the composite material, and adding silicone oil and flame retardant, the mechanical properties of the material and flame retardant properties are improved, and the bond strength and interface interaction between the resin matrix and the fiber are improved.

Benefits of technology

It significantly improves the wear resistance and flame retardant properties of composite materials, extends service life, and enhances its safety and mechanical properties under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909392A_ABST
    Figure CN118909392A_ABST
Patent Text Reader

Abstract

The invention discloses a wear-resistant resin-based composite material and a preparation method thereof, and relates to the technical field of composite material preparation, the composite material comprises the following raw materials by weight: 40-50 parts of thermosetting resin, 5-10 parts of a curing agent, 0.6-1 part of a lubricant, 3-8 parts of a flame retardant, and 1-3 parts of a filler; the lubricant is silicone oil, and the curing agent is selected from any one of phthalic anhydride, pyromellitic dianhydride, tetrahydrophthalic anhydride and maleic anhydride. According to the wear-resistant resin-based composite material and the preparation method thereof, the wear resistance of the composite material can be obviously improved by adding the modified silicon carbide whiskers, and meanwhile, the interface bonding strength of the silicon carbide whiskers and a resin matrix can be improved by modifying the silicon carbide whiskers through the silane coupling agent, so that the mechanical property of the composite material is improved; meanwhile, by adding the flame retardant, the flame retardant property of the composite material can be effectively improved, and the safety of the composite material in use under a high-temperature condition is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material preparation, in particular to a wear-resistant resin-based composite material and a preparation method thereof. Background Art

[0002] Resin-based composite materials are fiber-reinforced materials with organic polymers as the matrix, usually using glass fiber, carbon fiber, basalt fiber or aramid fiber reinforcement. Resin-based composite materials are widely used in aviation, automobile and marine industries.

[0003] The Chinese patent with the publication number CN105694355A discloses a resin-based composite material, which is made of the following raw materials in parts by weight: 90 parts of thermosetting resin, 5-8 parts of plastic additives, 15-25 parts of chopped glass fibers, 25-30 parts of mica powder, 1-3 parts of silane coupling agents, 5-8 parts of polyethylene, and 0.2-0.8 parts of catalysts, wherein the thermosetting resin is selected from one of phenolic resin, epoxy resin, and unsaturated polyester resin, and the plastic additives added in proportion during the preparation are subjected to pressure molding. The invention reduces the production cost while having good insulation performance, easy molding and manufacturing performance, and the stability of the material is greatly improved, and the anti-pollution and anti-corrosion properties are excellent, and it is widely used in various complex working conditions. However, the wear resistance of the resin-based composite material prepared by the above scheme is insufficient, which leads to the fact that after a period of use, it is very easy to be worn, thereby causing damage and affecting its service life; for this reason, the present invention provides a wear-resistant resin-based composite material and a preparation method thereof to solve the above problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a wear-resistant resin-based composite material and a preparation method thereof, which solves the problems mentioned in the above background technology.

[0005] To achieve the above objectives, the present invention is implemented by the following technical solutions: a wear-resistant resin-based composite material and a preparation method thereof, the composite material comprising the following raw materials in parts by weight: 40 to 50 parts of a thermosetting resin, 5 to 10 parts of a curing agent, 0.6 to 1 part of a lubricant, 3 to 8 parts of a flame retardant, and 1 to 3 parts of a filler;

[0006] The lubricant is silicone oil, the curing agent is selected from any one of phthalic anhydride, pyromellitic anhydride, tetrahydrophthalic anhydride and maleic anhydride, and the filler includes the following raw materials in weight percentage: 35% to 55% of modified silicon carbide whiskers and 40% to 65% of carbon fibers.

[0007] Preferably, the modification method of the modified silicon carbide whisker is:

[0008] S1, preparing a mixed solution of deionized water and anhydrous ethanol;

[0009] S2, then pour 0.2-0.5 mL of silane coupling agent into the mixed solution, and perform ultrasonic cleaning for 10-20 min;

[0010] S3, placing 2 to 5 g of silicon carbide whiskers in the solution, and stirring at a temperature of 45 to 50° C. for 30 to 50 min;

[0011] S4. Place the mixture in a drying oven and dry it at a constant temperature of 80 to 85°C for 3 to 4 hours to obtain modified silicon carbide whiskers.

[0012] Preferably, in S1, the volume ratio of deionized water to anhydrous ethanol is 1:1.

[0013] Preferably, in S2, the silane coupling agent is selected from one of KH550 and KH560.

[0014] Preferably, the preparation method of the flame retardant is: 100 g of N, N-bis (2-hydroxyethyl) amino methylene phosphonic acid diethyl ester and 50 mL of ethyl acetate are added to 100 g of tetrabromophthalic anhydride in sequence, nitrogen is introduced and stirred, and then poured into a rotary evaporator to obtain tetrabromophthalic acid (2-hydroxyethyl phosphonic acid diethyl ester methylene) amino mono-2-ethyl ester, which is the flame retardant.

[0015] Preferably, the stirring temperature is 80-90°C, the stirring time is 3.5-4.5h; and the rotary evaporation temperature is 45-55°C.

[0016] Preferably, the thermosetting resin is selected from any one of phenolic resin, epoxy resin and unsaturated polyester resin.

[0017] A method for preparing a wear-resistant resin-based composite material comprises the following preparation steps:

[0018] Step 1, pre-treating the carbon fiber for standby use;

[0019] Step 1: Add curing agent, flame retardant and lubricant to the thermosetting resin and mix them thoroughly;

[0020] Step 2: Add modified silicon carbide whiskers and pretreated carbon fibers and continue stirring;

[0021] Step 4: Pour the mixed material into a three-roll grinder and mix it evenly at room temperature, then vacuum it to remove bubbles, and finally pour it into a mold for curing, and demould it after cooling to obtain a wear-resistant resin-based composite material.

[0022] Preferably, the carbon fiber pretreatment method is: immersing the carbon fiber in a 5% by mass NaOH solution, then placing it in a drying oven for heat treatment, and finally washing it in deionized water and drying it;

[0023] The heat treatment temperature is 400-450°C, and the heat treatment time is 40-60 minutes.

[0024] Preferably, in step 4, the material is first cured at room temperature for 8 to 9 hours, then cured at 60 to 70° C. for 3.5 to 4.5 hours, and finally heated to 100 to 110° C. for 1 to 1.5 hours.

[0025] Beneficial Effects

[0026] The present invention provides a wear-resistant resin-based composite material and a preparation method thereof. Compared with the prior art, it has the following beneficial effects:

[0027] (1) The wear-resistant resin-based composite material and its preparation method can significantly improve the wear resistance of the composite material by adding modified silicon carbide whiskers. At the same time, the silicon carbide whiskers are modified by a silane coupling agent to enhance the interfacial bonding strength between the silicon carbide whiskers and the resin matrix, thereby improving the mechanical properties of the composite material. At the same time, the flame retardant can be added to effectively improve the flame retardant properties of the composite material, improve its safety when used under high temperature conditions, and thus extend the service life of the composite material.

[0028] (2) The wear-resistant resin-based composite material and its preparation method pretreat the surface of the carbon fiber to remove the organic glue on the surface, so that the surface of the carbon fiber has a certain degree of roughness, reduce the polarity of the fiber surface, and enhance the mechanical anchoring effect between the carbon fiber and the resin matrix, so that it can better combine with the resin and can also be more fully impregnated with the resin, thereby further increasing the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The surface morphology SEM images of carbon fibers before and after alkali treatment provided by the wear-resistant resin-based composite material and the preparation method thereof of the present invention;

[0030] Figure 2 Friction and wear performance test provided for a wear-resistant resin-based composite material and a preparation method thereof of the present invention;

[0031] Figure 3 A salt spray corrosion test provided for a wear-resistant resin-based composite material and a preparation method thereof of the present invention;

[0032] Figure 4 A scanning electron microscope image of a carbon layer of a resin-based composite material after combustion, provided by the present invention for a wear-resistant resin-based composite material and a preparation method thereof. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the technical scheme, the preparation method of the flame retardant is: to 100g of tetrabromophthalic anhydride, 100g of N, N-bis (2-hydroxyethyl) amino methylene phosphonic acid diethyl ester and 50mL of ethyl acetate are added in sequence, nitrogen is introduced and stirred at a temperature of 85°C for 4h, and then poured into a rotary evaporator at 50°C to obtain tetrabromophthalic acid (2-hydroxyethyl phosphonic acid diethyl ester methylene) amino mono-2-ethyl ester, which is the flame retardant.

[0035] Example 1

[0036] A wear-resistant resin-based composite material and a preparation method thereof, comprising the following preparation steps:

[0037] Step 1: pretreat the carbon fiber: immerse the carbon fiber in a 5% by mass NaOH solution, then place it in a drying oven at 400°C for 40 minutes, and finally wash it in deionized water and dry it;

[0038] Step 2: Add 10 g of phthalic anhydride, 8 g of flame retardant and 1 g of silicone oil to 40 g of thermosetting resin and mix thoroughly;

[0039] Step 3: Add 1.2 g of modified silicon carbide whiskers and 1.8 g of pretreated carbon fibers, and continue stirring;

[0040] The modification method of modified silicon carbide whiskers is:

[0041] S1. Prepare a mixed solution of deionized water and anhydrous ethanol in a volume ratio of 1:1;

[0042] S2, then pour 0.2 mL of KH550 into the mixed solution and perform ultrasonic cleaning for 10 min;

[0043] S3, placing 2 g of silicon carbide whiskers in the solution and stirring at 45° C. for 30 min;

[0044] S4, placing in a drying oven, and drying at a constant temperature of 80°C for 3 hours to obtain modified silicon carbide whiskers;

[0045] Step 4: Pour the mixed material into a three-roll grinder and mix it evenly at room temperature, then evacuate the mixture to remove bubbles, and finally pour it into a mold for curing. First, cure it at room temperature for 8 hours, then place it at 60°C for curing for 3.5 hours, and finally heat it to 100°C, cure it for 1 hour, and demold it after cooling to obtain a wear-resistant resin-based composite material.

[0046] Example 2

[0047] A wear-resistant resin-based composite material and a preparation method thereof, comprising the following preparation steps:

[0048] Step 1: pretreat the carbon fiber: immerse the carbon fiber in a 5% by mass NaOH solution, then place it in a drying oven at 450°C for heat treatment for 50 minutes, and finally wash it in deionized water and dry it;

[0049] Step 2: Add 8 g of pyromellitic anhydride, 6 g of flame retardant and 0.8 g of silicone oil to 45 g of thermosetting resin and mix thoroughly;

[0050] Step 3: Add 1g of modified silicon carbide whiskers and 1g of pretreated carbon fibers, and continue stirring;

[0051] The modification method of modified silicon carbide whiskers is:

[0052] S1. Prepare a mixed solution of deionized water and anhydrous ethanol in a volume ratio of 1:1;

[0053] S2, then pour 0.4 mL of KH550 into the mixed solution and perform ultrasonic cleaning for 15 min;

[0054] S3, placing 2.5 g of silicon carbide whiskers in the solution, and stirring at 50° C. for 30 to 50 minutes;

[0055] S4, placing in a drying oven, and drying at a constant temperature of 85°C for 4 hours to obtain modified silicon carbide whiskers;

[0056] Step 4: Pour the mixture into a three-roll grinder and mix it evenly at room temperature, then evacuate the mixture to remove bubbles, and finally pour it into a mold for curing. First, cure it at room temperature for 8 hours, then cure it at 65°C for 4 hours, and finally heat it to 1.5°C and cure it for 1.5 hours. After cooling, demold it to obtain a wear-resistant resin-based composite material.

[0057] Example 3

[0058] A wear-resistant resin-based composite material and a preparation method thereof, comprising the following preparation steps:

[0059] Step 1: pretreat the carbon fiber: immerse the carbon fiber in a 5% by mass NaOH solution, then place it in a drying oven at 450°C for 60 minutes, and finally wash it in deionized water and dry it;

[0060] Step 2: Add 5 g of maleic anhydride, 3 g of flame retardant and 0.6 g of silicone oil to 50 g of thermosetting resin and mix thoroughly;

[0061] Step 3: Add 0.55 g of modified silicon carbide whiskers and 0.45 g of pretreated carbon fibers, and continue stirring;

[0062] The modification method of modified silicon carbide whiskers is:

[0063] S1. Prepare a mixed solution of deionized water and anhydrous ethanol in a volume ratio of 1:1;

[0064] S2, then pour 0.5 mL of KH560 into the mixed solution and perform ultrasonic cleaning for 20 min;

[0065] S3, placing 5 g of silicon carbide whiskers in the solution and stirring at 50° C. for 50 min;

[0066] S4, placing in a drying oven, and drying at a constant temperature of 85°C for 4 hours to obtain modified silicon carbide whiskers;

[0067] Step 4: Pour the mixed material into a three-roll grinder and mix it evenly at room temperature, then evacuate the mixture to remove bubbles, and finally pour it into a mold for curing. First, cure it at room temperature for 9 hours, then place it at 70°C for curing for 4.5 hours, and finally heat it to 110°C and cure it for 1.5 hours. After cooling, demold it to obtain a wear-resistant resin-based composite material.

[0068] Comparative Example 1

[0069] A wear-resistant resin-based composite material and a preparation method thereof, comprising the following preparation steps:

[0070] Step 1: Add 10 g of phthalic anhydride, 8 g of diammonium phosphite and 1 g of silicone oil to 40 g of thermosetting resin and mix thoroughly;

[0071] Step 2: Add 1.2 g of silicon carbide whiskers and 1.8 g of carbon fiber and continue stirring;

[0072] Step 3: Pour the mixture into a three-roll grinder and mix it evenly at room temperature, then evacuate the mixture to remove bubbles, and finally pour it into a mold for curing. First, cure it at room temperature for 8 hours, then cure it at 60°C for 3.5 hours, and finally heat it to 100°C and cure it for 1 hour. After cooling, demold it to obtain a wear-resistant resin-based composite material.

[0073] Friction and wear performance test: The test was conducted using a ball-disc friction and wear tester. The friction mode was reciprocating motion under ball-plane contact. The friction pair was a quenched and tempered GCr15 stainless steel ball with a diameter of 4 mm. The friction load was 12 N and the wear time was 60 min. Other friction and wear test conditions were: room temperature, dry friction, and a reciprocating frequency of 2 Hz. Before the experiment, the sample surface was polished smooth with 800% iC water sandpaper, and the sample and the grinding ball surface were cleaned with a soft cloth soaked in alcohol and then dried. The friction coefficient was automatically recorded by the friction tester. The cross-sectional profile of the wear scar was measured using a roughness tester and the wear rate was calculated. The wear rate results are shown in Table 1, and the calculation formula is:

[0074] Where: W is the wear rate, %; F is the normal load, N; L is the total sliding length, m; ΔΔV is the volume wear, mm 3

[0075] Table 1

[0076] Wear rate / % Example 1 47.3 Example 2 23.4 Example 3 24.1 Comparative Example 1 23.9

[0077] like Figure 2 As shown in Table 1, the friction coefficient and wear rate of the samples of Examples 1-3 are significantly reduced compared with those of Comparative Example 1.

[0078] Combustion performance test: Tested using a cone calorimeter with a thermal radiation flux of 35kW / m 2 , the sample size is 100mm x 100mm x 3mm.

[0079] Mechanical properties test: According to GB-T1040.3-2006 standard, the tensile strength (Rb) and elongation at break (At) of the sample were measured using a universal mechanical testing machine at a tensile rate of 200 mm / min; the sample size was 30 mm x 30 mm x 2 mm; the results are shown in Table 2:

[0080] Table 2

[0081] <![CDATA[Tensile strength / MPa > Elongation at break / % Example 1 53.59 136 Example 2 52.86 129 Example 3 53.48 132 Comparative Example 1 26.74 98

[0082] Salt spray corrosion test: The sample was subjected to salt spray test in YWX / Q-150 salt spray test chamber, and salt spray aging test was carried out in accordance with GJB150.11A-2009. The experimental data of the sample during the salt spray process were recorded. The experimental conditions are shown in Table 3:

[0083] Table 3

[0084] Test conditions parameter Mass fraction of salt solution 5%±1% Test temperature (35±2)℃ pH of salt solutions 6.5~7.2 Salt spray deposition rate 1~3mL(80cm·h) Duration of the trial Alternate 24h salt spray and 24h drying

[0085] like Figure 3 As shown: From the uncorroded samples, it can be seen that there are potholes on the resin surface of the sample of comparative example 1. This is because the resin itself is relatively viscous, and there will still be bubbles after stirring in the resin tank, and its fluidity is poor, so bubbles will be generated when poured into the mold, so the surface of the prepared sample has potholes, while the uncorroded sample surfaces of Examples 1-3 basically do not show bubbling; after the salt spray test, the samples of Examples 1-3 do not have resin degumming or resin deficiency, indicating that the resin has strong copolymerization ability and good adhesion with the filler, thereby showing better corrosion resistance, while the sample of comparative example 1 can obviously see that the resin has degummed due to corrosion and partially fallen off.

[0086] like Figure 4 As shown: the carbon layer on the surface of the sample in comparative example 1 has poor continuity and exists a large number of voids, which fails to effectively isolate the heat exchange between the composite material and the external environment. Oxygen and combustibles can continue to exchange through the voids, thereby increasing the thermal release of the composite material. The carbon layer formed after the samples in embodiments 1-3 are burned is relatively dense and continuous, which can effectively prevent the heat exchange between the composite material and the external environment, reduce the mass loss of the material during combustion, prevent the escape of toxic and harmful gases, and improve the flame retardant properties of the composite material.

[0087] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0088] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A wear-resistant resin-based composite material, characterized in that: The composite material comprises the following raw materials in parts by weight: 40-50 parts of thermosetting resin, 5-10 parts of curing agent, 0.6-1 part of lubricant, 3-8 parts of flame retardant, and 1-3 parts of filler; The lubricant is silicone oil, the curing agent is selected from any one of phthalic anhydride, pyromellitic anhydride, tetrahydrophthalic anhydride and maleic anhydride, and the filler includes the following raw materials in weight percentage: 35% to 55% of modified silicon carbide whiskers and 40% to 65% of carbon fibers.

2. A wear-resistant resin-based composite material according to claim 1, characterized in that: The modification method of the modified silicon carbide whisker: S1, preparing a mixed solution of deionized water and anhydrous ethanol; S2, then pour 0.2-0.5 mL of silane coupling agent into the mixed solution, and perform ultrasonic cleaning for 10-20 min; S3, placing 2 to 5 g of silicon carbide whiskers in the solution, and stirring at a temperature of 45 to 50° C. for 30 to 50 min; S4. Place the mixture in a drying oven and dry it at a constant temperature of 80 to 85°C for 3 to 4 hours to obtain modified silicon carbide whiskers.

3. A wear-resistant resin-based composite material according to claim 2, characterized in that: In S1, the volume ratio of deionized water to anhydrous ethanol is 1:

1.

4. The wear-resistant resin-based composite material according to claim 2, characterized in that: In the S2, the silane coupling agent is selected from one of KH550 and KH560.

5. The wear-resistant resin-based composite material according to claim 1, characterized in that: The preparation method of the flame retardant is as follows: 100 g of N, N-bis (2-hydroxyethyl) amino methylene phosphonic acid diethyl ester and 50 mL of ethyl acetate are sequentially added into 100 g of tetrabromophthalic anhydride, nitrogen is introduced and stirred, and then the mixture is poured into a rotary evaporator to obtain tetrabromophthalic acid (2-hydroxyethyl phosphonic acid diethyl methylene) amino mono-2-ethyl ester, which is the flame retardant.

6. The wear-resistant resin-based composite material according to claim 5, characterized in that: The stirring temperature is 80-90°C, and the stirring time is 3.5-4.5h; the rotary evaporation temperature is 45-55°C.

7. The wear-resistant resin-based composite material according to claim 1, characterized in that: The thermosetting resin is selected from any one of phenolic resin, epoxy resin and unsaturated polyester resin.

8. A method for preparing the wear-resistant resin-based composite material according to claim 7, characterized in that: The method comprises the following preparation steps: Step 1, pre-treating the carbon fiber for standby use; Step 2: Add curing agent, flame retardant and lubricant to the thermosetting resin and mix them thoroughly; Step 3, adding modified silicon carbide whiskers and pretreated carbon fibers, and continuing to stir; Step 4: pour the mixed material into a three-roll grinder and mix it evenly at room temperature, then evacuate the mixture to remove bubbles, and finally pour it into a mold for curing, and demould it after cooling to obtain a wear-resistant resin-based composite material.

9. The method for preparing a wear-resistant resin-based composite material according to claim 8, characterized in that: The carbon fiber pretreatment method is as follows: immersing the carbon fiber in a 5% by mass NaOH solution, then placing the carbon fiber in a drying oven for heat treatment, and finally washing and drying the carbon fiber in deionized water; The heat treatment temperature is 400-450°C, and the heat treatment time is 40-60 minutes.

10. The method for preparing a wear-resistant resin-based composite material according to claim 8, characterized in that: In the step 4, the material is first cured at room temperature for 8 to 9 hours, then cured at 60 to 70° C. for 3.5 to 4.5 hours, and finally heated to 100 to 110° C. for 1 to 1.5 hours.

Citation Information

Patent Citations

  • Silicon carbide whisker-modified nylon engineering plastic

    CN104559142A

  • Reactive flame retardant applied to polyurethane materials and preparation method of reactive flame retardant

    CN105646813A