Matt PCABS composite material and preparation method thereof
By using phosphorus-based flame retardants, inorganic nano-micro powders and polyurethane foam in matte PCABS composites, the problem of poor flame retardant effect is solved, better flame retardant, heat resistance and heat insulation performance are achieved, and the material is enhanced protection performance.
Patent Information
- Application Number
- CN202411206723.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
AI Technical Summary
Matt PCABS composites have poor flame retardant effects in the presence of fire, resulting in damage and lack of flame retardant protection.
The matte PCABS composite material is prepared by drying, mixing, extruding, cooling and drying steps, enhancing its flame retardant, heat resistance and heat insulation properties.
It improves the flame retardancy, heat resistance and heat insulation of matte PCABS composite materials, enhances its protective performance during use, and avoids spontaneous combustion and damage.
Smart Images

Figure CN118909419A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of matte PCABS composite materials, and in particular to a matte PCABS composite material and a preparation method thereof. Background Art
[0002] Matte PCABS composite material is usually a composite material mixed with polycarbonate and two materials. Polycarbonate has excellent heat and weather resistance, dimensional stability and impact resistance. At the same time, engineering plastic alloy has excellent processing fluidity. Therefore, matte PCABS composite material has excellent comprehensive properties, including excellent impact strength, good dimensional stability, electrical properties, wear resistance, chemical resistance and dyeing resistance, and has good molding and machining.
[0003] Matte PCABS composite materials are widely used, but when matte PCABS composite materials are used, if there is a fire, the matte PCABS composite materials will have poor flame retardant effect, resulting in damage to the matte PCABS composite materials, and therefore it is necessary for matte PCABS composite materials to have flame retardancy. Summary of the invention
[0004] The object of the present invention is to provide a matte PCABS composite material and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a matte PCABS composite material, characterized in that it comprises the following components in parts by mass:
[0006] Polycarbonate resin 80.0-85.0 parts;
[0007] ABS resin 12.0-30.0 parts;
[0008] Thermoplastic elastomer 6.0-15.0 parts;
[0009] Epoxy polymer 4.0-20.0 parts;
[0010] 4.0-15.0 parts of high-glue powder;
[0011] Antioxidant 0.1-1.8 parts;
[0012] 2.0-10.0 parts of organic matte agent;
[0013] 2.0-5.0 parts of inorganic matte agent;
[0014] Flame retardant 2.0-4.0 parts;
[0015] 3.0-6.0 parts of toughening agent;
[0016] Heat-resistant agent 2.0-4.0 parts;
[0017] 3.0-7.0 parts of heat insulation agent;
[0018] Lubricant 0.1-1.5 parts.
[0019] Preferably, the polycarbonate resin is at least one of aromatic polycarbonates having a viscosity average molecular weight of 10,000 to 40,000.
[0020] Preferably, the antioxidant is an aromatic amine antioxidant, and the lubricant is liquid paraffin.
[0021] Preferably, the flame retardant is a phosphorus-based flame retardant, and the heat-resistant agent is an inorganic nanopowder.
[0022] Preferably, the thermal insulation agent is polyurethane foam.
[0023] A method for preparing a matte PCABS composite material, characterized by comprising the following specific steps:
[0024] Step 1: Weigh the respective portions of polycarbonate resin, ABS resin, thermoplastic elastomer, epoxy polymer, high rubber powder, antioxidant, organic matting agent, inorganic matting agent, flame retardant, toughening agent, heat resistant agent, heat insulating agent and lubricant of matte PCABS composite material by weighing equipment, and place the corresponding components at the same time;
[0025] Step 2: Place each component into the drying equipment for drying;
[0026] Step 3: Add each component into the interior of the mixing device in sequence, and then the mixing device stirs and mixes the multiple components until they are evenly mixed, thereby obtaining a premix;
[0027] Step 4: putting the premix obtained after stirring into the interior of the extruder, and then making the extruder perform extrusion, and at the same time using a pelletizing device to perform granulation treatment;
[0028] Step 5: placing the granulated material into a cooling device for cooling, and taking it out after cooling;
[0029] Step 6: Use drying equipment to dry the cooled granulated material to obtain a matte PCABS composite material.
[0030] Preferably, the drying temperature of the drying equipment in step 2 is 100-140 degrees Celsius, and the drying time is 10-20 hours.
[0031] Preferably, the extrusion equipment in step 4 is a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 110-180 degrees Celsius.
[0032] Preferably, the mixing equipment in step three is a high-speed stirrer, and the rotation speed of the high-speed stirrer is 280-320 rpm.
[0033] Preferably, the drying time of the drying equipment in step six is 3-6 hours.
[0034] Technical effects and advantages of the present invention:
[0035] The present invention utilizes a flame retardant, a heat-resistant agent and a heat-insulating agent in a coordinated arrangement. The flame retardant is a phosphorus-based flame retardant, thereby making the matte PCABS composite material flame retardant. Meanwhile, the heat-resistant agent is an inorganic nano-powder and the heat-insulating agent is a polyurethane foam. The heat-resistant agent and the heat-insulating agent make the matte PCABS composite material heat-resistant and heat-insulating, thereby facilitating flame retardancy, heat insulation and heat-resistant protection of the matte PCABS composite material, and facilitating flame retardancy protection of the matte PCABS composite material during use. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The figure is a schematic diagram of the preparation process of the matte PCABS composite material of the present invention. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Embodiment 1
[0039] The present invention provides Figure 1 A matte PCABS composite material shown, comprising the following components by weight:
[0040] 80.0-85.0 parts of polycarbonate resin, 12.0-30.0 parts of ABS resin, 6.0-15.0 parts of thermoplastic elastomer, 4.0-20.0 parts of epoxy polymer, 4.0-15.0 parts of high-glue powder, 0.1-1.8 parts of antioxidant, the main function of which is to inhibit or delay the oxidative degradation reaction of the polymer, thereby protecting the physical and mechanical properties and appearance properties such as color and smell of the polymer, 2.0-10.0 parts of organic matting agent, 2.0-5.0 parts of inorganic matting agent, 2.0-4.0 parts of flame retardant, 3.0-6.0 parts of toughening agent, the main function of which is to improve the toughness of the polymer, thereby helping to improve the toughness of the matte PCABS composite material, 2.0-4.0 parts of heat resistant agent, 3.0-7.0 parts of heat insulating agent, and 0.1-1.5 parts of lubricant.
[0041] The polycarbonate resin is at least one kind of aromatic polycarbonate having a viscosity average molecular weight of 10,000 to 40,000.
[0042] The antioxidant adopts aromatic amine antioxidant, the lubricant adopts liquid paraffin, which is a colorless, transparent, oily liquid. It does not show fluorescence under sunlight and is odorless and tasteless at room temperature. The lubricant is beneficial to increase the smoothness of the matte PCABS composite material. The flame retardant adopts phosphorus flame retardant. Phosphorus flame retardant mainly achieves flame retardant effect by forming an isolation film between the material and the oxidant and heat source. The moisture generated by phosphorus flame retardant in the flame retardant process can not only reduce the temperature of the condensed phase, but also dilute the concentration of combustibles in the gas phase, thereby achieving a good flame retardant effect. According to the different flame retardant effects of phosphorus compounds in different reaction zones, The flame retardant mechanism is divided into condensed phase flame retardant mechanism and gas phase flame retardant mechanism. Flame retardants are beneficial to improve the flame retardancy of matte PCABS composite materials, and are convenient for flame retardant protection of matte PCABS composite materials during use to avoid the occurrence of combustion-supporting and other situations. Heat-resistant agents use inorganic nanopowders. The flame retardant effects of inorganic nanopowders include catalytic inhibition, heat insulation, heat absorption and physical shielding. The catalytic inhibition effect is that inorganic nanopowders can be used as catalysts to catalyze the decomposition of free radicals in polymer materials and inhibit the initiation and propagation of chain reactions, thereby effectively slowing down and inhibiting the combustion process of polymers. The heat insulation effect is that inorganic nanopowders Micropowders have a high specific surface area and can form a dense protective film on the surface of polymer materials, effectively isolating oxygen and heat, reducing heat conduction and heat radiation, and thus preventing the combustion of polymers. The endothermic effect is that inorganic nanopowders have a high specific surface area and good heat absorption properties, which can absorb and transfer heat to the surrounding environment, reduce the surface temperature of polymer materials, and thus slow down the combustion process. The physical shielding effect is that inorganic nanopowders can be evenly dispersed in polymer materials to form a physical barrier that hinders the spread of flames and the transfer of heat, thereby inhibiting the combustion of polymers. Inorganic nanopowders are wear-resistant and heat-resistant. It is beneficial to make the matte PCABS composite material wear-resistant and heat-resistant. The heat-resistant agent is beneficial to increase the heat resistance of the matte PCABS composite material, which is beneficial to the matte PCABS composite material for self-heat protection to avoid random spontaneous combustion. The heat-insulating agent adopts polyurethane foam. Polyurethane foam is a lightweight, high-strength thermal insulation material with excellent thermal insulation effect and high compression resistance. The heat-insulating agent is beneficial to increase the thermal insulation of the matte PCABS composite material, which is beneficial to the thermal insulation protection of the interior of the matte PCABS composite material, so as to improve the performance of the matte PCABS composite material.
[0043] A method for preparing a matte PCABS composite material, comprising:
[0044] The various portions of polycarbonate resin, ABS resin, thermoplastic elastomer, epoxy polymer, high rubber powder, antioxidant, organic matting agent, inorganic matting agent, flame retardant, toughening agent, heat resistant agent, heat insulating agent and lubricant of the matte PCABS composite material are weighed by weighing equipment, and the corresponding components are placed at the same time.
[0045] Each component is placed in a drying device for drying. The drying temperature of the drying device is 100-140 degrees Celsius and the drying time is 10-20 hours.
[0046] Each component is added into the interior of the mixing device in sequence. The mixing device is a high-speed stirrer. The speed of the high-speed stirrer is 280-320 rpm. Then the mixing device stirs and mixes the multiple components until they are evenly mixed. At this time, a premix is obtained.
[0047] The premix obtained after stirring is put into the interior of the extrusion equipment, which is a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 110-180 degrees Celsius. Then the extrusion equipment is extruded, and a pelletizing device is used for granulation treatment.
[0048] The granulated material is placed in a cooling device for cooling and taken out after cooling.
[0049] The cooled granulated material is dried using a drying device with a drying time of 3-6 hours to obtain a matte PCABS composite material.
[0050] Embodiment 2
[0051] A matte PCABS composite material comprises the following components in parts by mass: 80.0-85.0 parts of polycarbonate resin, 12.0-30.0 parts of ABS resin, 6.0-15.0 parts of thermoplastic elastomer, 4.0-20.0 parts of epoxy polymer, 4.0-15.0 parts of high-glue powder, 0.1-1.8 parts of antioxidant, 2.0-10.0 parts of organic matte agent, 2.0-5.0 parts of inorganic matte agent, 3.0-6.0 parts of toughening agent and 0.1-1.5 parts of lubricant.
[0052] The polycarbonate resin is at least one kind of aromatic polycarbonate having a viscosity average molecular weight of 10,000 to 40,000.
[0053] A method for preparing a matte PCABS composite material, comprising:
[0054] The various portions of polycarbonate resin, ABS resin, thermoplastic elastomer, epoxy polymer, high rubber powder, antioxidant, organic matting agent, inorganic matting agent, flame retardant, toughening agent, heat resistant agent, heat insulating agent and lubricant of the matte PCABS composite material are weighed by weighing equipment, and the corresponding components are placed at the same time.
[0055] Each component is placed in a drying device for drying. The drying temperature of the drying device is 100-140 degrees Celsius and the drying time is 10-20 hours.
[0056] Add each component to the interior of the mixing equipment in turn. The mixing equipment is a high-speed mixer. The high-speed mixer can quickly mix various raw materials together, thereby improving production efficiency. The high-speed mixer has uniformity. The high-speed mixer can make the raw materials mix more evenly, thereby ensuring product quality and reliability. The high-speed mixer adopts advanced mixing technology, which can ensure long-term stable operation and reduce failure rate. The high-speed mixer is adjustable. The mixing speed and mixing time of the high-speed mixer can be adjusted as needed to meet different production needs. It is easy to operate. The operation of the high-speed mixer is simple and easy to understand, and it is convenient for employees to use and maintain. The speed of the high-speed mixer is 280-320 rpm. Then the mixing equipment stirs and mixes multiple components until they are evenly mixed, and a premix is obtained at this time.
[0057] The premix obtained after stirring is put into the interior of the extrusion equipment, which is a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 110-180 degrees Celsius. Then the extrusion equipment is extruded, and a pelletizing device is used for granulation treatment.
[0058] The granulated material is placed in a cooling device for cooling and taken out after cooling.
[0059] The cooled granulated material is dried using a drying device, which is beneficial for drying the granulated material. The drying time of the drying device is 3-6 hours. After drying, a matte PCABS composite material can be obtained.
[0060] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A matte PCABS composite material, characterized in that: By mass, it includes the following components: Polycarbonate resin 80.0-85.0 parts; ABS resin 12.0-30.0 parts; Thermoplastic elastomer 6.0-15.0 parts; Epoxy polymer 4.0-20.0 parts; 4.0-15.0 parts of high-glue powder; Antioxidant 0.1-1.8 parts; 2.0-10.0 parts of organic matte agent; 2.0-5.0 parts of inorganic matte agent; Flame retardant 2.0-4.0 parts; 3.0-6.0 parts of toughening agent; Heat-resistant agent 2.0-4.0 parts; 3.0-7.0 parts of heat insulation agent; Lubricant 0.1-1.5 parts.
2. A matte PCABS composite material according to claim 1, characterized in that: The polycarbonate resin is at least one of aromatic polycarbonates having a viscosity average molecular weight of 10,000 to 40,000.
3. A matte PCABS composite material according to claim 1, characterized in that: The antioxidant is an aromatic amine antioxidant, and the lubricant is liquid paraffin.
4. A matte PCABS composite material according to claim 1, characterized in that: The flame retardant is a phosphorus-based flame retardant, and the heat-resistant agent is an inorganic nano powder.
5. The matte PCABS composite material according to claim 1, characterized in that: The heat insulating agent adopts polyurethane foam.
6. A method for preparing a matte PCABS composite material, characterized in that: The specific steps include: Step 1: Weigh the respective portions of polycarbonate resin, ABS resin, thermoplastic elastomer, epoxy polymer, high rubber powder, antioxidant, organic matting agent, inorganic matting agent, flame retardant, toughening agent, heat resistant agent, heat insulating agent and lubricant of matte PCABS composite material by weighing equipment, and place the corresponding components at the same time; Step 2: Place each component into the drying equipment for drying; Step 3: Add each component into the interior of the mixing device in sequence, and then the mixing device stirs and mixes the multiple components until they are evenly mixed, thereby obtaining a premix; Step 4: putting the premix obtained after stirring into the interior of the extruder, and then making the extruder perform extrusion, and at the same time using a pelletizing device to perform granulation treatment; Step 5: placing the granulated material into a cooling device for cooling, and taking it out after cooling; Step 6: Use drying equipment to dry the cooled granulated material to obtain a matte PCABS composite material.
7. The method for preparing a matte PCABS composite material according to claim 6, characterized in that: The drying temperature of the drying equipment in step 2 is 100-140 degrees Celsius, and the drying time is 10-20 hours.
8. The method for preparing a matte PCABS composite material according to claim 6, characterized in that: The extrusion equipment in step 4 is a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 110-180 degrees Celsius.
9. The method for preparing a matte PCABS composite material according to claim 6, characterized in that: The mixing equipment in step 3 is a high-speed mixer, and the rotation speed of the high-speed mixer is 280-320 revolutions per minute.
10. The method for preparing a matte PCABS composite material according to claim 6, characterized in that: The drying time of the drying equipment in step 6 is 3-6 hours.