High-temperature-resistant wear-resistant self-lubricating pulley and preparation method thereof

By combining polyaryletherketone with ultra-high molecular weight polyethylene and inorganic filler, combined with high-temperature pressing and extrusion processes, the problem of insufficient wear resistance and thermal conductivity of plastic pulleys in high-temperature environments is solved, and the pulleys are high-temperature resistance and high-temperature resistance Abrasive and self-lubricating properties are suitable for special areas of distinguishing between high temperature and color.

CN118909424APending Publication Date: 2024-11-08NINGBO MAYBACH ENG PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410620455.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing plastic pulleys are not able to resist wear and thermal conductivity in high temperature environments, and cannot be used in special areas where color distinction is required, and mechanical damage and noise problems are prone to long-term use.

Method used

Polyaryletherketone materials are combined with ultra-high molecular weight polyethylene and inorganic fillers (such as alumina and magnesium oxide), and high-temperature wear-resistant self-lubricating pulleys are prepared through high-temperature pressing and extrusion processes to increase the thermal conductivity and hardness of the material. And improve performance with lubricants and antioxidants.

Benefits of technology

It realizes wear resistance, self-lubricity and high thermal conductivity of pulley sliding at a high speed under 200℃, extends service life and reduces noise, and is suitable for high-temperature environments and color distinction needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant wear-resistant self-lubricating pulley and a preparation method thereof. The high-temperature-resistant wear-resistant self-lubricating pulley comprises the following components in percentage by mass: 40%-90% of polyaryletherketone, 1%-20% of ultra-high molecular weight polyethylene, 5%-40% of inorganic filler, 0.1%-2% of a lubricant, 0.1%-2% of an antioxidant and 0.1%-2% of a coupling agent. The friction coefficient and the volume wear rate of the polyaryletherketone are reduced by using the ultra-high molecular weight polyethylene, and the heat-conducting property and the high-temperature resistance of the polyaryletherketone are improved by using the inorganic filler, so that the prepared pulley can be used at a high temperature (gt; and in addition, the high-wear-resistance, self-lubricating and high-heat-conduction performances are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermoplastic polymer material modification, and in particular to a high-temperature-resistant and wear-resistant self-lubricating pulley and a preparation method thereof. Background Art

[0002] Pulleys can save effort and change the direction of force. At present, pulleys play a vital role in the fields of mechanical processing and assembly. Pulleys are mainly divided into two types: plastic pulleys and metal pulleys. High-performance plastic pulleys have become the first choice to replace metal pulleys. Therefore, in addition to basic wear resistance and high hardness, high-performance plastic pulleys also need to have low friction coefficient, high temperature resistance, high thermal conductivity, and free color matching to meet the use conditions in various working environments.

[0003] Currently, commonly used plastic pulleys are made of modified polyamide and modified polyoxymethylene materials. The friction coefficient or wear of nylon is reduced by adding wear-resistant additives such as carbon fiber, glass fiber, molybdenum disulfide, graphite, polytetrafluoroethylene powder or silicone powder to the resin. However, this type of plastic pulley has limitations: (1) Due to the heat resistance of materials such as polyamide and polyoxymethylene, the heat resistance of composite materials is not high, and the long-term use temperature is generally limited to below 150°C; (2) Fillers such as carbon fiber, molybdenum dioxide, and graphite added to polymers can improve the wear resistance of the material, but can only be used to prepare black products, which cannot be used in certain special fields, such as aerospace, emergency rescue, etc., where the parts required in some links are similar in material and shape but different in function and need to be distinguished by color; (3) Glass fiber can produce a strong mechanical bond between polymers, and can also improve the comprehensiveness of plastic structures, improve bearing capacity and wear resistance. Because there is a "floating fiber" phenomenon between glass fiber and plastic, a small amount of High-rigidity glass fiber will be exposed on the outer surface of the plastic, causing serious wear of the matching parts used with the pulley; (4) When the pulley works for a long time, the friction heat will cause the pulley to heat up. The metal pulley has a high melting point and strong thermal conductivity, which can dissipate local heat to the entire pulley, avoiding local damage to the pulley. However, the plastic pulley does not have as high thermal conductivity as the metal pulley, and the heat of the pulley (generally the part where the pulley is directly in contact with the matching part) will be too high. In this case, the plastic pulley with low heat resistance and low thermal conductivity is very likely to be mechanically damaged at the heated part, shortening the service life of the pulley; (5) The pulley will make an abnormal noise when working. The sound is caused by vibration. Excessive size gap will cause noise due to vibration when the pulley is working. Therefore, the dimensional stability of the pulley is very important. The size of polyamide material is greatly affected by moisture; (6) Polyoxymethylene (POM) material is rich in formaldehyde, which will release formaldehyde when heated for a long time, and it is easy to become powdery during operation, with serious powder loss.

[0004] In addition to having a low surface friction coefficient and high hardness, wear-resistant plastics must also have self-lubricating properties. Although lubricants can be added to the surface of the product, lubricants have many disadvantages. Over time, the grease will age and require regular maintenance. It is easy to accumulate dust and debris, contaminating internal parts, etc. Therefore, plastic pulleys with good wear resistance and self-lubrication are the best choice.

[0005] Polyaryletherketoneketone is a type of crystalline polymer formed by connecting phenylene rings through oxygen bridges (ether bonds) and carbonyl groups (ketones). High temperature resistance is one of the most prominent advantages of polyaryletherketone. The long-term use temperature is as high as 260°C, the instantaneous use temperature can reach 300°C, and it hardly decomposes in a short time at 400°C, which is much higher than ordinary engineering plastics. Compared with other high-temperature resistant plastics such as polyimide (PI), polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polyphenylene ether (PPO), etc., the upper limit of the long-term use temperature of PEEK is nearly 50°C higher.

[0006] Polyaryletherketone resin has outstanding tribological properties, certain self-lubricating properties, low friction coefficient, and low wear rate. It is a good wear-resistant plastic, but it cannot be used in occasions with strict wear resistance requirements. Due to the low thermal conductivity of polyaryletherketone material itself, when sliding at high speed on the iron metal dual surface, when a certain critical temperature or heat dissipation rate is reached, the friction power consumption will rise very quickly, and the friction dual parts will suffer serious chemical and mechanical damage, which limits the application of polyaryletherketone in high-speed sliding occasions. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the technical defects of the background technology and provide a high temperature resistant, wear-resistant and self-lubricating pulley and a preparation method thereof. In order to design a high temperature resistant, wear-resistant and self-lubricating pulley, the present invention provides a polyaryletherketone pulley, which can be used for high-speed sliding in a 200°C environment for a long time, and has the properties of wear resistance, self-lubrication, noise reduction and high thermal conductivity. In addition, the present invention increases the dispersibility of inorganic fillers through improvements on the process end.

[0008] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0009] A high temperature resistant and wear resistant self-lubricating pulley comprises the following components in percentage by mass:

[0010]

[0011] Preferably, the polyaryletherketone is selected from any one or more of polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK) and polyetherketoneetherketoneketone (PEKEKK).

[0012] Preferably, the average viscosity average molecular weight of the ultra-high molecular weight polyethylene is in the range of 4×10 6 ~6×10 6 Between g / mol.

[0013] Preferably, the mesh size of the inorganic filler is greater than 5000 mesh; the inorganic filler is selected from any one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, and boron nitride.

[0014] Preferably, the lubricant is selected from any one or more of zinc stearate, Fischer-Tropsch wax, and pentaerythritol stearate (PETS).

[0015] Preferably, the antioxidant is selected from any one or more of antioxidant 1010, antioxidant 168, antioxidant 1076, and antioxidant 1098.

[0016] Preferably, the coupling agent is selected from any one or both of an aluminate coupling agent and a titanate coupling agent.

[0017] The present invention also provides a method for preparing the high temperature resistant and wear resistant self-lubricating pulley as described above, comprising the following steps:

[0018] (1) Weighing an inorganic filler and a coupling agent according to a weight ratio, putting them into a high-speed mixer, and mixing them evenly;

[0019] (2) Weighing polyaryletherketone powder, ultra-high molecular weight polyethylene, lubricant, and antioxidant according to weight ratio, putting them into a high-speed mixer, and mixing them evenly;

[0020] (3) taking out the mixed material from step (2), placing it on a mold, and pressing it into a plate at high temperature;

[0021] (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0022] (5) placing the granules in step (4) in a co-rotating twin-screw extruder, extruding and granulating to obtain blended granules;

[0023] (6) placing the blended pellets obtained in step (5) in an injection molding machine and performing injection molding to obtain a high temperature resistant and wear resistant self-lubricating pulley.

[0024] Preferably, in step (1), the high-speed mixer is set at 100 to 600 rpm, the temperature is set at 80 to 200° C., and the high-speed stirring is performed for 5 to 30 min.

[0025] Preferably, in step (2), the high-speed mixer is set at 100 to 600 rpm, the temperature is set at 80 to 200° C., and the high-speed stirring is performed for 3 to 15 minutes.

[0026] Preferably, in step (3), the plate is pressed at high temperature to a thickness of 5 mm, the molding temperature is 350-400° C., and the molding time is 0.5-4 h.

[0027] Preferably, in step (5), the extruder speed is set at 100-400 rpm, the extrusion temperature is set at 350-400°C, and the die temperature is set at 340-390°C.

[0028] Preferably, in step (6), the injection molding machine barrel temperature is 360-400°C, and the injection nozzle temperature is 350-390°C.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) Ultra-high molecular weight polyethylene (UHMWPE) has the characteristics of wear resistance, low friction coefficient, self-lubrication, etc. It is a self-lubricating material on the surface of a non-sticky substrate. The friction coefficient is only 0.07-0.11, and the sliding wear resistance is very excellent. It is particularly suitable for use in the sliding wear resistance field, such as pulley products. The present invention uses UHMWPE as a friction modifier for polyaryletherketone, which further improves the wear resistance of polyaryletherketone resin.

[0031] (2) Ultra-high molecular weight polyethylene (UHMWPE) has excellent impact energy absorption, and its impact energy absorption value is the highest among all plastics. Therefore, it has good noise damping performance and excellent sound reduction effect, which can improve the noise reduction performance of polyaryletherketone;

[0032] (3) Since the surface hardness of UHMWPE is relatively low, it will weaken the surface hardness of the polyaryletherketone composite material. Therefore, the inorganic filler added in the present invention can make up for the defect and improve the surface hardness of the composite material;

[0033] (4) The inorganic filler added in the present invention not only plays a role in supporting and bearing and reducing deformation, but also can transfer the polymer film, improve the adhesion strength of the transfer film, reduce friction, and reduce wear;

[0034] (5) The thermal conductivity of PEEK at room temperature is only 0.25W / (m·K). When the PEEK pulley slides at high speed, heat will be generated. If the heat cannot be discharged in time, it will cause chemical and mechanical damage to the friction part of the pulley. The inorganic fillers such as aluminum oxide and magnesium oxide of the present invention can form a heat conduction channel inside the PPEK resin, increase the thermal conductivity of the PEEK composite pulley, and avoid damage caused by the heat generated by the high-speed sliding of the pulley cannot be dissipated;

[0035] (6) The particle size of inorganic fillers is small, the bulk density is very small, the powder is fluffy, and the volume occupies a large proportion. If the powder and plastic particles are physically mixed and then directly put into a twin-screw extruder for blending, it will lead to uneven mixing of materials and serious powder agglomeration. Therefore, the present invention uses polyaryletherketone micropowder to replace polyaryletherketone pellets. The inorganic powder and the resin powder are first physically mixed and evenly pressed into a plate, and then crushed and melt-mixed for the second time using a twin-screw extruder. This approach avoids the problems of dust loss caused by large volume of powder, unstable feeding during the granulation process, and uneven powder dispersion. DETAILED DESCRIPTION

[0036] In order to better understand the content of the present invention, further description is given below in conjunction with specific embodiments. It should be understood that these embodiments are only used to further illustrate the present invention, and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content described in the present invention, those skilled in the art make some non-essential changes or adjustments to the present invention, which still belong to the protection scope of the present invention.

[0037] Example 1

[0038] A high temperature resistant and wear resistant self-lubricating pulley, comprising the following components:

[0039]

[0040] The preparation method of the high temperature resistant and wear resistant self-lubricating pulley as described above comprises the following steps:

[0041] (1) Weigh alumina and aluminate coupling agent according to the weight ratio, put them into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 10 minutes;

[0042] (2) PEEK powder, ultra-high molecular weight polyethylene, zinc stearate, and antioxidant 1010 were weighed according to weight ratio, put into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 5 min;

[0043] (3) The mixed material in step (2) is taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature is 370° C. and the molding time is 1 h.

[0044] (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0045] (5) placing the particles in step (4) in a co-rotating twin-screw extruder, setting the extruder speed to 200 rpm, the extrusion temperature to 370° C., and the die temperature to 360° C. to obtain blended pellets;

[0046] (6) The blended pellets obtained in step (5) are placed in an injection molding machine with a barrel temperature of 380° C. and an injection nozzle temperature of 370° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0047] The PEEK powder used in this embodiment was purchased from Solvay Company with the brand name KT-820FP; the ultra-high molecular weight polyethylene was purchased from Celanese Company with the brand name 2126, average viscosity average molecular weight is 4.2×10 6 g / mol; alumina powder particle size 6250 mesh.

[0048] Example 2

[0049] A high temperature resistant and wear resistant self-lubricating pulley, comprising the following components:

[0050]

[0051] The preparation method of the high temperature resistant and wear resistant self-lubricating pulley as described above comprises the following steps:

[0052] (1) Weigh alumina and aluminate coupling agent according to the weight ratio, put them into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 10 minutes;

[0053] (2) PEEK powder, ultra-high molecular weight polyethylene, zinc stearate, and antioxidant 1010 were weighed according to weight ratio, put into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 5 min;

[0054] (3) The mixed material in step (2) is taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature is 370° C. and the molding time is 1 h.

[0055] (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0056] (5) placing the particles in step (4) in a co-rotating twin-screw extruder, setting the extruder speed to 200 rpm, the extrusion temperature to 370° C., and the die temperature to 360° C. to obtain blended pellets;

[0057] (6) The blended pellets obtained in step (5) are placed in an injection molding machine with a barrel temperature of 380° C. and an injection nozzle temperature of 370° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0058] The PEEK powder used in this embodiment was purchased from Solvay Company with the brand name KT-820FP; the ultra-high molecular weight polyethylene was purchased from Celanese Company with the brand name 2126, average viscosity average molecular weight is 4.2×10 6 g / mol; alumina powder particle size 6250 mesh.

[0059] Example 3

[0060] A high temperature resistant and wear resistant self-lubricating pulley, comprising the following components:

[0061]

[0062] The method for preparing a high temperature resistant, wear resistant and self-lubricating pulley as described above comprises the following steps:

[0063] (1) Weigh alumina and aluminate coupling agent according to the weight ratio, put them into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 10 minutes;

[0064] (2) PEEK powder, ultra-high molecular weight polyethylene, zinc stearate, and antioxidant 1010 were weighed according to weight ratio, put into a high-speed mixer, set the high-speed mixer at 200 rpm, set the temperature at 100° C., and stir at high speed for 5 min;

[0065] (3) The mixed material in step (2) is taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature is 370° C. and the molding time is 1 h.

[0066] (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0067] (5) placing the particles in step (4) in a co-rotating twin-screw extruder, setting the extruder speed to 200 rpm, the extrusion temperature to 370° C., and the die temperature to 360° C. to obtain blended pellets;

[0068] (6) The blended pellets obtained in step (5) are placed in an injection molding machine with a barrel temperature of 380° C. and an injection nozzle temperature of 370° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0069] The PEEK powder used in this embodiment was purchased from Solvay Company with the brand name KT-820FP; the ultra-high molecular weight polyethylene was purchased from Celanese Company with the brand name 2126, average viscosity average molecular weight is 4.2×10 6 g / mol; alumina powder particle size 6250 mesh.

[0070] Example 4

[0071] A high temperature resistant and wear resistant self-lubricating pulley, comprising the following components:

[0072]

[0073] The preparation method of the high temperature resistant and wear resistant self-lubricating pulley as described above comprises the following steps:

[0074] (1) Weigh magnesium oxide and titanate coupling agent according to weight ratio, put into a high-speed mixer, set the high-speed mixer at 300 rpm, set the temperature at 110° C., and stir at high speed for 12 minutes;

[0075] (2) PEK powder, ultra-high molecular weight polyethylene, PETS, and antioxidant 168 were weighed according to the weight ratio, and put into a high-speed mixer. The high-speed mixer was set at 300 rpm and the temperature was set at 110° C., and stirred at high speed for 5 minutes;

[0076] (3) The mixed material in step (2) was taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature was 380° C. and the molding time was 1.2 h.

[0077] (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0078] (5) placing the particles in step (4) in a co-rotating twin-screw extruder, setting the extruder speed to 250 rpm, the extrusion temperature to 390° C., and the die temperature to 380° C. to obtain blended pellets;

[0079] (6) The blended pellets obtained in step (5) are placed in an injection molding machine with a barrel temperature of 390° C. and an injection nozzle temperature of 380° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0080] The PEK powder used in this example was purchased from Victrex Company and its brand is HT TM P45PF; ultra-high molecular weight polyethylene purchased from Celanese Company, brand 4022, average viscosity average molecular weight is 5×10 6 g / mol; magnesium oxide powder particle size 8000 mesh.

[0081] Comparative Example 1

[0082] A method for preparing a pulley, comprising the following steps:

[0083] (1) Weigh 100 kg of PEEK powder and put it into a high-speed mixer. Set the high-speed mixer to 200 rpm, the temperature to 100 °C, and stir at high speed for 5 min;

[0084] (2) The material of step (1) is taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature is 370° C. and the molding time is 1 h.

[0085] (3) crushing the plate pressed in step (2) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0086] (4) placing the particles in step (3) in a co-rotating twin-screw extruder, setting the extruder speed to 200 rpm, the extrusion temperature to 370° C., and the die temperature to 360° C. to obtain blended pellets;

[0087] (5) The blended pellets obtained in step (4) are placed in an injection molding machine with a barrel temperature of 380° C. and an injection nozzle temperature of 370° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0088] The PEEK powder used in this comparative example was purchased from Solvay Company with the brand name KT-820FP.

[0089] Comparative Example 2

[0090] A method for preparing a pulley, comprising the following steps:

[0091] (1) Weigh 100 kg of PEK powder and put it into a high-speed mixer. Set the high-speed mixer to 300 rpm, the temperature to 110 °C, and stir at high speed for 12 min;

[0092] (2) The material of step (1) was taken out, placed on a mold, and pressed at high temperature into a plate with a thickness of 5 mm. The molding temperature was 380° C. and the molding time was 1.2 h.

[0093] (3) crushing the plate pressed in step (2) and screening out particles with a maximum diameter of less than 4 mm using a sieve;

[0094] (4) placing the particles in step (3) in a co-rotating twin-screw extruder, setting the extruder speed to 250 rpm, the extrusion temperature to 390° C., and the die temperature to 380° C. to obtain blended pellets;

[0095] (5) The blended pellets obtained in step (4) are placed in an injection molding machine with a barrel temperature of 390° C. and an injection nozzle temperature of 380° C., and are injection molded into standard specimens and pulleys, and various properties are tested using the standard specimens.

[0096] The PEK powder used in this comparative example was purchased from Victrex Company and its brand is HTTM P45PF.

[0097] Table 1 Summary of test data of pulleys prepared in Examples 1 to 4 and Comparative Examples 1 to 2

[0098]

[0099] By comparing the data of Example 1 and Example 2 in the test table, it can be found that the increase in the content of ultra-high molecular weight polyethylene can significantly reduce the friction coefficient and volume wear rate. By comparing Example 1 and Example 3, it can be found that the increase in inorganic filler can improve the hardness, heat deformation temperature, and thermal conductivity of the composite material, and then reduce the volume wear rate. It can be seen from the data of the examples and comparative examples that the use of ultra-high molecular weight polyethylene and inorganic fillers can maintain the excellent mechanical properties of polyaryletherketone while improving the thermal conductivity, wear resistance, and high temperature resistance of polyaryletherketone resin.

[0100] The present invention selects ultra-high molecular weight polyethylene to reduce the friction coefficient and volume wear rate of polyaryletherketone, and increases the thermal conductivity and high temperature resistance of polyaryletherketone through inorganic fillers, so that the prepared pulley can be used for a long time at high temperature (>160°C) and has the properties of high wear resistance, self-lubrication and high thermal conductivity.

[0101] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.

Claims

1. A high temperature resistant and wear resistant self-lubricating pulley, It is characterized in that The components include the following mass percentages:

2. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The polyaryletherketone is selected from any one or more of polyetheretherketone, polyetherketone, polyetherketoneketone, polyetheretherketoneketone and polyetherketoneetherketoneketone.

3. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The average viscosity-average molecular weight of the ultra-high molecular weight polyethylene is in the range of 4×106 to 6×106 g / mol.

4. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The mesh number of the inorganic filler is greater than 5000 mesh; the inorganic filler is selected from any one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, and boron nitride.

5. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The lubricant is selected from any one or more of zinc stearate, Fischer-Tropsch wax, and pentaerythritol stearate.

6. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The antioxidant is selected from any one or more of antioxidant 1010, antioxidant 168, antioxidant 1076, and antioxidant 1098.

7. A high temperature resistant and wear resistant self-lubricating pulley as claimed in claim 1, It is characterized in that The coupling agent is selected from any one or both of an aluminate coupling agent and a titanate coupling agent.

8. A method for preparing a high temperature resistant and wear resistant self-lubricating pulley according to any one of claims 1 to 7, It is characterized in that The steps include: (1) Weighing an inorganic filler and a coupling agent according to a weight ratio, putting them into a high-speed mixer, and mixing them evenly; (2) Weighing polyaryletherketone powder, ultra-high molecular weight polyethylene, lubricant, and antioxidant according to weight ratio, putting them into a high-speed mixer, and mixing them evenly; (3) taking out the mixed material from step (2), placing it on a mold, and pressing it into a plate at high temperature; (4) crushing the plate pressed in step (3) and screening out particles with a maximum diameter of less than 4 mm using a sieve; (5) placing the granules in step (4) in a co-rotating twin-screw extruder, extruding and granulating to obtain blended granules; (6) placing the blended pellets obtained in step (5) in an injection molding machine and performing injection molding to obtain a high temperature resistant and wear resistant self-lubricating pulley.

9. A method for preparing a high temperature resistant and wear resistant self-lubricating pulley according to claim 8, It is characterized in that In step (1), the high-speed mixer is set at 100-600 rpm, the temperature is set at 80-200° C., and the high-speed stirring is performed for 5-30 min; in step (2), the high-speed mixer is set at 100-600 rpm, the temperature is set at 80-200° C., and the high-speed stirring is performed for 3-15 min.

10. A method for preparing a high temperature resistant and wear resistant self-lubricating pulley according to claim 8, It is characterized in that In step (3), a plate with a thickness of 5 mm is pressed at high temperature, the molding temperature is 350-400° C., and the molding time is 0.5-4 h; in step (5), the extruder speed is set at 100-400 rpm, the extrusion temperature is set at 350-400° C., and the die head temperature is set at 340-390° C.; in step (6), the injection molding machine barrel temperature is 360-400° C., and the injection nozzle temperature is 350-390° C.