Preparation method and application of composite material tunnel bridge

By combining modified boron nitride nanosheets and carbon oxide fibers, a thermal conductivity network is formed and material compatibility is improved, which solves the problems of low thermal conductivity and easy foam structure of composite tunnel trays, and achieves efficient heat dissipation and flame retardant performance The improvement is suitable for high-performance tunnel tray applications.

CN118909428APending Publication Date: 2024-11-08JIANGXI LONGZHENG TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134990.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing composite tunnel bridges have low thermal conductivity and easy foam structure of polyurethane polymers, resulting in insufficient thermal conductivity and difficult to meet the requirements of efficient heat dissipation and flame retardant.

Method used

Modified boron nitride nanosheets and carbon oxide fibers are used to combine them to form a thermal conductivity network and improve material compatibility, thereby improving the heat dissipation and flame retardant properties of the material. Modified boron nitride nanosheets are modified by surface activation and silane coupling agent to enhance their dispersion and mechanical properties in polymers, and reduce foam structure through surface modification of carbon oxidation fibers, improving overall thermal conductivity and flame retardant performance.

Benefits of technology

It has achieved the improvement of efficient heat dissipation and flame retardant performance of composite materials, and significantly improved bending strength, ultimate oxygen index and thermal conductivity, making it suitable for high-performance tunnel tray applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909428A_ABST
    Figure CN118909428A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a composite material tunnel bridge stand, the preparation method comprises the following steps: S1, uniformly mixing 90 parts by weight of a polyurethane polymer, 20-30 parts by weight of modified boron nitride nanosheets, 3-7 parts by weight of carbon oxide fibers, 18-28 parts by weight of a plasticizer, 5-10 parts by weight of a compatilizer, 1-2 parts by weight of an antioxidant and 0.5-1 part by weight of a lubricant, putting the mixture into an internal mixer, and carrying out extrusion molding to obtain a composite material tunnel bridge stand; the rotor speed of the internal mixer is 40 r / min, the internal mixing temperature is 175-180 DEG C, and the internal mixing time is 8-10 min; s2, feeding the internally mixed material obtained in the step S1 into a double-screw extruder, and performing extrusion granulation at 170-185 DEG C to obtain a composite material; and S3, feeding the composite material obtained in the S2 into an injection molding machine, melting at 175-185 DEG C, injecting into a mold, and cooling to obtain the composite material tunnel bridge. According to the invention, the material prepared by taking the polyurethane polymer as the matrix is excellent in mechanical property, and also has high flame retardance and high thermal conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a preparation method and application of a composite material tunnel bridge. Background Art

[0002] With the rapid development and progress of science and technology, the materials, functions and use effects of tunnel bridges have also made great progress. The bridges installed in tunnels are mainly used to support and protect power cables, control cables, lighting cables and their accessories. In tunnels, underpasses, urban rail transit and other places, bridges play an important role. The bridge can prevent the cable from mechanical damage, such as extrusion and impact, to ensure the integrity and safety of the cable. Through the bridge system, various cables can be classified and arranged in layers to make the cable lines more orderly and easy to maintain and manage. The design of the bridge usually takes into account the heat dissipation problem to ensure that the heat generated by the cable during operation can be effectively dissipated to avoid overheating affecting the performance of the cable. The bridge system can be flexibly designed according to the actual direction and spatial conditions of the tunnel to adapt to different installation environments. In the event of natural disasters such as earthquakes, the bridge system can also provide certain seismic support to reduce losses. By installing the bridge on the ceiling or wall of the tunnel, the ground space can be saved, the internal space of the tunnel can be more reasonably utilized, and the cables can be hidden so that the cables are not exposed to the outside, making the interior of the tunnel more beautiful, while also reducing the accumulation of dust and dirt.

[0003] Existing composite materials are used to make tunnel bridges. Since the composite materials use polyurethane polymer as the matrix, polyurethane polymer is an elastomer with properties between plastic and rubber. Although it has good oil resistance, wear resistance, aging resistance and low temperature resistance, compared with materials such as metals, polyurethane has a lower thermal conductivity, which means that its heat transfer capacity is limited and is not conducive to heat dissipation. Since the polyurethane molecular chain contains a large number of organic soft segments and hard segments, and the interaction between the molecular chains is strong, the internal heat transfer mainly relies on the vibration and collision of the molecular chain, which is less efficient. In addition, polyurethane polymers are prone to produce foam structures during processing. Although this structure is conducive to buffering and heat preservation, it will further reduce the thermal conductivity of the material. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a preparation method and application of a composite material tunnel bridge, ensuring that the material made with polyurethane polymer as the matrix has excellent mechanical properties while also having high flame retardancy and high thermal conductivity.

[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for preparing a composite material tunnel bridge, comprising the following steps:

[0006] S1. Mix 90 parts of polyurethane polymer, 20-30 parts of modified boron nitride nanosheets, 3-7 parts of oxidized carbon fibers, 18-28 parts of plasticizer, 5-10 parts of compatibilizer, 1-2 parts of antioxidant and 0.5-1 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 175-180°C, and the internal mixing time is 8-10min to obtain an internal mixing material;

[0007] S2, feeding the mixed material obtained in S1 into a twin-screw extruder, and extruding and granulating the material at 170-185° C. to obtain a composite material;

[0008] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 175-185°C, injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0009] Furthermore, the preparation method of the modified boron nitride nanosheets is as follows:

[0010] A1. Dissolve 20-25 parts by weight of boron nitride nanosheets in 5 mol / L NaOH solution, and stir in an oil bath at 120° C. for 20 h to 22 h to obtain a mixture;

[0011] A2, filtering the mixture obtained in A1, washing the solids for several times, filtering them by suction until they are neutral, and drying them in an oven at 90° C. for 6 h to obtain activated boron nitride nanosheets with increased surface hydroxyl groups;

[0012] A3, prepare solution a by mixing 7-9 parts of acetone with 1 part of hydrochloric acid solution with pH=3, dissolve 2-3 parts of modifier in solution a, and hydrolyze in a 55°C water bath for 30 minutes to obtain solution b, then add the activated boron nitride nanosheets obtained in A2 to solution b, stir for 3 hours, and then dry in an oven at 100°C to obtain modified boron nitride nanosheets.

[0013] Furthermore, the modifier is a silane coupling agent.

[0014] Furthermore, in A1, the boron nitride nanosheets are 22 parts, and stirred in an oil bath at 120° C. for 20 h to obtain a mixture.

[0015] Further, in A3, 9 parts of acetone and 1 part of hydrochloric acid solution with pH=3 are prepared into solution a, 3 parts of modifier are dissolved in solution a, and hydrolyzed in a 55°C water bath for 30 minutes to obtain solution b.

[0016] Furthermore, the preparation method of the oxidized carbon fiber is as follows:

[0017] B1. Boil the carbon fiber with distilled water for 2 hours to remove impurities to obtain purified carbon fiber;

[0018] B2. Take the purified carbon fiber obtained in B1, put it into a round-bottom flask, add concentrated nitric acid and concentrated sulfuric acid in a ratio of 3:1, heat in a water bath at 60°C for 4 hours, filter, wash until neutral, and dry to obtain oxidized carbon fiber.

[0019] Furthermore, the plasticizer includes one of tricresyl phosphate, tributyl phosphate, and diisononyl phthalate, or a mixture of at least two of them.

[0020] Furthermore, the antioxidant includes a phenolic antioxidant or an amine antioxidant.

[0021] Furthermore, the lubricant includes a fatty acid lubricant or a fatty acid ester lubricant.

[0022] In a second aspect, the present invention provides an application of a composite tunnel bridge, wherein the composite tunnel bridge is prepared by the above-mentioned preparation method, and the composite tunnel bridge is applied in a tunnel as a structure for carrying cables and pipelines.

[0023] This application has the following beneficial effects:

[0024] 1. The present invention adopts modified boron nitride nanosheets, which can form a highly connected thermal conductive network in the composite material matrix. This thermal conductive network helps heat to be transferred along the high thermal conductive filler (oxidized carbon fiber), thereby realizing efficient heat transmission; the modified boron nitride nanosheets and oxidized carbon fibers are used in combination, and the two work together to construct a more complete thermal conductive path at multiple scales, thereby synergistically improving the overall heat dissipation performance.

[0025] 2. In the preparation of modified boron carbide nanosheets, activated boron nitride nanosheets rich in hydroxyl groups on the surface are obtained by filtering, rinsing to neutrality and then drying, which provide active sites for subsequent surface modification. Silane coupling agents are combined in the form of covalent bonds to improve the compatibility and dispersibility of boron nitride nanosheets in polymer matrices or other media. On the one hand, the mechanical properties of the material are more effectively improved; on the other hand, the interfacial thermal resistance between the filler and the polyurethane polymer is reduced, and by providing a more ordered lattice structure, the scattering of phonons is reduced and the heat conduction efficiency is improved; the modified boron nitride nanosheets have a stable physical structure at high temperatures and can form a dense barrier layer when the polymer burns to prevent heat transfer and oxygen diffusion, thereby playing a flame retardant role. At the same time, the modified boron nitride nanosheets can promote the formation of a continuous and dense carbon layer on the polymer surface. This carbon layer can effectively isolate oxygen and combustible gases, reduce the combustion rate of the material, and significantly improve the limiting oxygen index of the material.

[0026] 3. In the preparation of oxidized carbon fiber, the surface roughness of the carbon fiber is improved through surface modification technology, the mechanical anchoring effect with the polymer is increased, air entrapment is reduced, and the proportion of foam structure that is easily generated by polyurethane polymers during processing is reduced, effectively avoiding the decrease in the thermal conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 , a comparative trend chart of the bending strength test data of the composite materials obtained in Examples 1-5 and Comparative Examples 1-6 in the test examples of the present invention;

[0028] Figure 2 , a comparative trend chart of limiting oxygen index test data of composite materials obtained in Examples 1-5 and Comparative Examples 1-6 in the test examples of the present invention;

[0029] Figure 3 , a comparative trend chart of thermal conductivity test data of composite materials obtained in Examples 1-5 and Comparative Examples 1-6 in the test examples of the present invention;

[0030] Figure 4 , a schematic diagram of the three-dimensional structure of one of the bridge frames of the present invention. DETAILED DESCRIPTION

[0031] The present application is further described in detail below with reference to the embodiments.

[0032] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0033] Example 1: (1) First, prepare modified boron nitride nanosheets, the steps are as follows:

[0034] A1. Dissolve 22 parts of boron nitride nanosheets in 5 mol / L NaOH solution by weight, until all the boron nitride nanosheets are immersed in the NaOH solution, i.e., no boron nitride nanosheets are exposed, and stir in an oil bath at 120° C. for 20 h to obtain a mixture.

[0035] A2. Filter the mixture obtained in A1, rinse the solid with deionized water for multiple times, filter until it is neutral, and bake in an oven at 90° C. for 6 h to obtain activated boron nitride nanosheets with increased surface hydroxyl groups.

[0036] A3. According to the same standard weight parts, 9 parts of acetone and 1 part of hydrochloric acid solution with pH = 3 are prepared into solution a, 3 parts of vinyltrimethoxysilane are dissolved in solution a, and hydrolyzed in a 55°C water bath for 30 minutes to obtain solution b, and then the activated boron nitride nanosheets obtained in A2 are added to solution b, stirred for 3 hours, and then dried in an oven at 100°C to obtain modified boron nitride nanosheets.

[0037] Among them, boron nitride nanosheets (10043-11-5) were purchased from Wuhan Kemik Biomedical Technology Co., Ltd. Vinyl trimethoxysilane (New Blue Sky LT-575) was purchased from Guangzhou Jingyi New Materials Co., Ltd.

[0038] (2) Then, the oxidized carbon fiber is prepared as follows:

[0039] B1. Boil the carbon fiber in distilled water for 2 hours to remove impurities and obtain purified carbon fiber.

[0040] B2. Take the purified carbon fiber obtained in B1, put it into a round-bottom flask, add a mixture of concentrated nitric acid and concentrated sulfuric acid in a mass ratio of 3:1 (enough to submerge the purified carbon fiber), heat in a 60°C water bath for 4 hours, filter, wash with deionized water several times until neutral, and dry to obtain oxidized carbon fiber.

[0041] Among them, carbon fiber (C6-4.0 / 240-T130) was purchased from Leisu Trading (Shanghai) Co., Ltd.

[0042] (3) Finally, the composite material tunnel bridge is prepared in the following steps:

[0043] S1. Mix 90 parts of polyurethane polymer, 25 parts of modified boron nitride nanosheets, 5 parts of oxidized carbon fibers, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40 r / min, the internal mixing temperature is 177° C., and the internal mixing time is 9 min to obtain an internal mixing material.

[0044] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0045] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0046] Among them, the polyurethane polymer (Utechllan USR55A) was purchased from Dongguan Jiurui Plastic Raw Materials Co., Ltd. The antioxidant is a phenolic antioxidant, specifically antioxidant 2246, which is a bisphenol structure antioxidant with the advantages of reduced volatility and better effect. The lubricant is specifically stearic acid. The compatibilizer (BP-1) was purchased from Coais Chemical Co., Ltd. The plasticizer is tricresyl phosphate (industrial grade), purchased from Jingzhou Yinjie Chemical Co., Ltd.

[0047] The composite material tunnel bridge prepared by the above method can be used in tunnels as a structure for carrying cables and pipelines.

[0048] Example 2: The difference between this example and Example 1 is that the modified boron nitride nanosheets are prepared in the following steps:

[0049] A1. Dissolve 20 parts by weight of boron nitride nanosheets in 5 mol / L NaOH solution until all the boron nitride nanosheets are immersed in the NaOH solution, and stir in an oil bath at 120° C. for 20 h to obtain a mixture.

[0050] A2. Filter the mixture obtained in A1, rinse the solid with deionized water for multiple times, filter until it is neutral, and bake in an oven at 90° C. for 6 h to obtain activated boron nitride nanosheets with increased surface hydroxyl groups.

[0051] A3. Prepare solution a by mixing 7 parts of acetone with 1 part of hydrochloric acid solution with a pH value of 3, dissolve 2 parts of vinyltrimethoxysilane in solution a, and hydrolyze in a water bath at 55°C for 30 minutes to obtain solution b, then add the activated boron nitride nanosheets obtained in A2 to solution b, stir for 3 hours, and then dry in an oven at 100°C to obtain modified boron nitride nanosheets.

[0052] Example 3: The difference between this example and Example 1 is that the modified boron nitride nanosheets are prepared in the following steps:

[0053] A1. Dissolve 25 parts of boron nitride nanosheets in 5 mol / L NaOH solution by weight until all the boron nitride nanosheets are immersed in the NaOH solution, and stir in an oil bath at 120° C. for 22 hours to obtain a mixture.

[0054] A2. Filter the mixture obtained in A1, rinse the solid with deionized water for multiple times, filter until it is neutral, and bake in an oven at 90° C. for 6 h to obtain activated boron nitride nanosheets with increased surface hydroxyl groups.

[0055] A3, 9 parts of acetone and 1 part of hydrochloric acid solution with pH = 3 are prepared into solution a, 3 parts of vinyltrimethoxysilane are dissolved in solution a, and hydrolyzed in a 55°C water bath for 30 minutes to obtain solution b, and then the activated boron nitride nanosheets obtained in A2 are added to solution b, stirred for 3 hours, and then dried in an oven at 100°C to obtain modified boron nitride nanosheets.

[0056] Embodiment 4: The difference between this embodiment and embodiment 1 is that the steps of preparing a composite material tunnel bridge are as follows:

[0057] S1. Mix 90 parts of polyurethane polymer, 20 parts of modified boron nitride nanosheets, 3 parts of oxidized carbon fibers, 18 parts of plasticizer, 5 parts of compatibilizer, 1 part of antioxidant and 0.5 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40 r / min, the internal mixing temperature is 175° C., and the internal mixing time is 8 min to obtain an internal mixing material.

[0058] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0059] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 175° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0060] Example 5: The difference between this example and Example 1 is that the steps for preparing a composite material tunnel bridge are as follows:

[0061] S1. Mix 90 parts of polyurethane polymer, 30 parts of modified boron nitride nanosheets, 7 parts of oxidized carbon fibers, 28 parts of plasticizer, 10 parts of compatibilizer, 2 parts of antioxidant and 1 part of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40 r / min, the internal mixing temperature is 180° C., and the internal mixing time is 10 min to obtain an internal mixing material.

[0062] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0063] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 185° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0064] Comparative Example 1: The difference between this comparative example and Example 1 is that in the preparation of the modified boron nitride nanosheets, the activation step is deleted, that is, the boron nitride nanosheets are directly modified without being activated.

[0065] The modified boron nitride nanosheets are prepared as follows: 9 parts of acetone and 1 part of hydrochloric acid solution with a pH of 3 are prepared into solution a, 3 parts of vinyltrimethoxysilane are dissolved in solution a, and hydrolyzed in a 55°C water bath for 30 minutes to obtain solution b, and then 22 parts of boron nitride nanosheets are added to solution b, stirred for 3 hours, and then dried in an oven at 100°C to obtain modified boron nitride nanosheets.

[0066] Comparative Example 2: The difference between this comparative example and Example 1 is that the modified boron nitride nanosheets are replaced by boron nitride nanosheets, that is, the boron nitride nanosheets are neither activated nor modified.

[0067] Specifically, the steps of preparing the composite material tunnel bridge are as follows:

[0068] S1. Mix 90 parts of polyurethane polymer, 25 parts of boron nitride nanosheets, 5 parts of oxidized carbon fibers, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40 r / min, the internal mixing temperature is 177° C., and the internal mixing time is 9 min to obtain an internal mixing material.

[0069] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0070] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0071] Comparative Example 3: The difference between this comparative example and Example 1 is that the modified boron nitride nanosheets are deleted.

[0072] Specifically, the steps of preparing the composite material tunnel bridge are as follows:

[0073] S1. Mix 90 parts of polyurethane polymer, 5 parts of oxidized carbon fiber, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 177°C, and the internal mixing time is 9min to obtain an internal mixing material.

[0074] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0075] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0076] Comparative Example 4: The difference between this comparative example and Example 1 is that the oxidized carbon fiber is replaced by carbon fiber.

[0077] Specifically, the steps of preparing the composite material tunnel bridge are as follows:

[0078] S1. Mix 90 parts of polyurethane polymer, 25 parts of modified boron nitride nanosheets, 5 parts of carbon fiber, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 177°C, and the internal mixing time is 9min to obtain an internal mixing material.

[0079] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0080] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0081] Comparative Example 5: The difference between this comparative example and Example 1 is that the oxidized carbon fiber is deleted.

[0082] Specifically, the steps of preparing the composite material tunnel bridge are as follows:

[0083] S1. Mix 90 parts of polyurethane polymer, 25 parts of modified boron nitride nanosheets, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 177°C, and the internal mixing time is 9min to obtain an internal mixing material.

[0084] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0085] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0086] Comparative Example 6: The difference between this comparative example and Example 1 is that the modified boron nitride nanosheets and oxidized carbon fibers are deleted.

[0087] Specifically, the steps of preparing the composite material tunnel bridge are as follows:

[0088] S1. Mix 90 parts of polyurethane polymer, 20 parts of plasticizer, 7 parts of compatibilizer, 1.4 parts of antioxidant and 0.9 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 177°C, and the internal mixing time is 9min to obtain an internal mixing material.

[0089] S2. The mixed material obtained in S1 is fed into a twin-screw extruder. The temperatures of each zone of the twin-screw extruder are set to 170°C, 170°C, 175°C, 180°C, 180°C, 185°C, 180°C, 175°C, and 170°C in sequence. The die temperature is 165°C, the screw speed is 110rpm, and extrusion granulation is performed to obtain a composite material.

[0090] S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 180° C., injected into a mold, and cooled to obtain a composite material tunnel bridge.

[0091] Test example: Test object: Composite materials were prepared according to Examples 1-5 and Comparative Examples 1-6.

[0092] Test items and basis / methods: 1. Flexural strength-ISO 178-2010, tested with a span of 64 mm and a speed of 2 mm / min.

[0093] 2. Limiting oxygen index-GB / T10707-2008.

[0094] 3. Thermal conductivity - Hot disk transient plane source method. A thermal constant analyzer (Hot Disk TPS2500S, Sweden) was used to quantitatively analyze the thermal conductivity of the composite materials. A disk with a radius of 25 mm and a thickness of 2 mm was used to measure the thermal conductivity at room temperature and in an air atmosphere.

[0095] Test results: See Table 1.

[0096] Table 1. Test data of the experimental example

[0097] Bending strength(MPa) Limiting oxygen index (%) Thermal conductivity (W / m·K) Example 1 120.7 31.4 1.13 Example 2 117.4 31.7 1.08 Example 3 119.8 30.1 1.15 Example 4 121.3 30.6 1.12 Example 5 123.5 32.2 1.12 Comparative Example 1 115.4 29.1 1.07 Comparative Example 2 106.7 26.3 1.01 Comparative Example 3 91.2 22.5 0.88 Comparative Example 4 116.2 30.4 0.99 Comparative Example 5 104.3 28.7 0.92 Comparative Example 6 85.8 20.6 0.79

[0098] Result analysis: Analyze examples 1-5 and combine the data in Table 1 and Figure 1-3 It can be seen that the composite material prepared by the present invention ensures that the polyurethane polymer is used as the matrix, and has excellent mechanical properties (bending strength is as high as 117.4 MPa or more), high flame retardancy (limiting oxygen index is as high as 30.1% or more) and high thermal conductivity (thermal conductivity coefficient is as high as 1.08 W / mK or more).

[0099] Analyze Example 1 and Comparative Examples 1-3 and combine the data in Table 1 and Figure 1-3It can be seen that the use of boron nitride nanosheets can improve the mechanical properties (bending strength), flame retardancy (limiting oxygen index) and thermal conductivity (thermal conductivity coefficient) of the composite materials; the improvement effect is enhanced by activating the boron nitride nanosheets to obtain activated boron nitride nanosheets and then using them; the improvement effect is further enhanced by silane-modifying the activated boron nitride nanosheets to obtain modified boron nitride nanosheets.

[0100] Analyze Example 1 and Comparative Examples 4-5 and combine the data in Table 1 and Figure 1-3 It can be seen that the use of carbon fiber can improve the mechanical properties (bending strength), flame retardancy (limiting oxygen index) and thermal conductivity (thermal conductivity coefficient) of the composite materials; the improvement effect is enhanced by oxidizing the carbon fiber to obtain oxidized carbon fiber and then using it.

[0101] Analyze Example 1 and Comparative Examples 3, 5 and 6 and combine the data in Table 1 and Figure 1-3 It can be seen that there is a synergistic effect between the modified boron nitride nanosheets and the oxidized carbon fibers, which can work synergistically to synergistically improve the mechanical properties (flexural strength), flame retardancy (limiting oxygen index) and thermal conductivity (thermal conductivity coefficient) of the prepared composite materials.

[0102] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0103] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a composite material tunnel bridge, It is characterized in that The steps include: S1. Mix 90 parts of polyurethane polymer, 20-30 parts of modified boron nitride nanosheets, 3-7 parts of oxidized carbon fibers, 18-28 parts of plasticizer, 5-10 parts of compatibilizer, 1-2 parts of antioxidant and 0.5-1 parts of lubricant by weight, and put them into an internal mixer. The rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 175-180°C, and the internal mixing time is 8-10min to obtain an internal mixing material; S2, feeding the mixed material obtained in S1 into a twin-screw extruder, and extruding and granulating the material at 170-185° C. to obtain a composite material; S3. The composite material obtained in S2 is fed into an injection molding machine, melted at 175-185°C, injected into a mold, and cooled to obtain a composite material tunnel bridge.

2. The method for preparing the composite material tunnel bridge according to claim 1, It is characterized in that The preparation method of the modified boron nitride nanosheets is as follows: A1. Dissolve 20-25 parts by weight of boron nitride nanosheets in 5 mol / L NaOH solution, and stir in an oil bath at 120° C. for 20 h to 22 h to obtain a mixture; A2, filtering the mixture obtained in A1, washing the solids for several times, filtering them by suction until they are neutral, and drying them in an oven at 90° C. for 6 h to obtain activated boron nitride nanosheets with increased surface hydroxyl groups; A3, prepare solution a by mixing 7-9 parts of acetone with 1 part of hydrochloric acid solution with pH=3, dissolve 2-3 parts of modifier in solution a, and hydrolyze in a 55°C water bath for 30 minutes to obtain solution b, then add the activated boron nitride nanosheets obtained in A2 to solution b, stir for 3 hours, and then dry in an oven at 100°C to obtain modified boron nitride nanosheets.

3. The method for preparing the composite material tunnel bridge according to claim 2, It is characterized in that The modifier is a silane coupling agent.

4. The method for preparing the composite material tunnel bridge according to claim 2, It is characterized in that In A1, the amount of boron nitride nanosheets was 22 parts, and the mixture was stirred in an oil bath at 120° C. for 20 hours to obtain a mixture.

5. The method for preparing the composite material tunnel bridge according to claim 2 or 4, It is characterized in that In A3, 9 parts of acetone and 1 part of hydrochloric acid solution with pH=3 are prepared into solution a, 3 parts of modifier are dissolved in solution a, and hydrolyzed in a 55°C water bath for 30 minutes to obtain solution b.

6. The method for preparing the composite material tunnel bridge according to claim 1, It is characterized in that The preparation method of the oxidized carbon fiber is as follows: B1. Boil the carbon fiber with distilled water for 2 hours to obtain purified carbon fiber; B2. Take the purified carbon fiber obtained in B1, put it into a round-bottom flask, add concentrated nitric acid and concentrated sulfuric acid in a ratio of 3:1, heat in a water bath at 60°C for 4 hours, filter, wash until neutral, and dry to obtain oxidized carbon fiber.

7. The method for preparing the composite material tunnel bridge according to claim 1, It is characterized in that The plasticizer includes one of tricresyl phosphate, tributyl phosphate and diisononyl phthalate or a mixture of at least two of them.

8. The method for preparing the composite material tunnel bridge according to claim 1, It is characterized in that The antioxidant includes a phenolic antioxidant or an amine antioxidant.

9. The method for preparing the composite material tunnel bridge according to claim 1, It is characterized in that The lubricant includes a fatty acid lubricant or a fatty acid ester lubricant.

10. Application of a composite material tunnel bridge, It is characterized in that The composite material tunnel bridge is prepared by the preparation method according to any one of claims 1 to 9, and the composite material tunnel bridge is used in a tunnel as a structure for carrying cables and pipelines.