Polyamide-polyether block polymer composite material as well as preparation method and application thereof

Through the preparation of polyamide-polyether block polymer composite materials, polyamide elastomers with functionalized polyolefins and nanocelluloses are combined with traditional moisture-permeable film materials. The poor virus effect and insufficient low-temperature performance have achieved excellent moisture permeability and mechanical performance of the material, and are suitable for a variety of application scenarios.

CN118909435APending Publication Date: 2024-11-08SHANDONG GUANGYIN NEW MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411126154.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional moisture permeable film materials have poor antibacterial and antiviral effects and lack low temperature performance, making it difficult to have excellent moisture permeability and mechanical properties at the same time.

Method used

Using polyamide-polyether block polymer composite material, the combination of polyamide elastomers containing high polyamide hard and polyether soft segments and functionalized polyolefins and nanocellulose is prepared with excellent moisture permeability and mechanical properties. Performance water-proof and moisture-permeable film material.

Benefits of technology

It has achieved the improvement of high moisture permeability and mechanical properties of the materials, and is suitable for textiles, packaging and medical fields, meeting the needs of different application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of moisture permeable film materials, in particular to a polyamide-polyether block polymer composite material and a preparation method and application thereof. The composite material is prepared from the following raw materials in parts by mass: 40-80 parts of polyamide elastomer, 10-50 parts of polyolefin, 5-20 parts of functionalized polyolefin and 0.1-5 parts of nano cellulose. The polyamide elastomer is a polymer composed of 70-90 parts by mass of a polyamide hard segment and 10-30 parts by mass of a polyether soft segment. The polyamide elastomer disclosed by the invention is high in hard segment content, and the prepared moisture-permeable film has excellent mechanical properties. The nanocellulose has good hydrophilicity, and the moisture permeability of the moisture-permeable film is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of moisture permeable membrane materials, and in particular to a polyamide-polyether block polymer composite material and a preparation method and application thereof. Background Art

[0002] Breathable membranes are mainly divided into porous breathable membranes and non-porous breathable membranes. The porous breathable membrane material is mainly polyolefin resin formed by heat stretching with pores of 0.01~10μm, which allows gas to pass but liquid cannot pass through. The water barrier depends on the pore size of the breathable membrane. Common viruses are generally 0.02~0.4μm in diameter, and bacteria are 0.2~50μm in size. Therefore, the antibacterial and antiviral effects of this type of film are poor, and there are potential risks in the application of medical and food packaging. The main representative of non-porous breathable membranes is TPU, which mainly conducts water vapor from one side with high concentration and high pressure to the other side through the hygroscopicity of hydrophilic groups. The principle is similar to that of water entering cells. It has a wide range of applications in clothing fabrics, medical care, nursing and other fields. However, the traditional TPU material has a low melting point of only about 120℃, large wet impedance, and poor low-temperature performance.

[0003] As a high-performance elastomeric material, polyamide-polyether block copolymer material has high elasticity, excellent mechanical properties, excellent biocompatibility, and excellent low temperature resistance. The amorphous polyether soft segment plays a major role in the air and moisture permeability as a hydrophilic group, while the crystalline polyamide hard segment plays a decisive role in the mechanical properties of the material. The increase of the polyether portion will improve the moisture permeability of the material, but it will inevitably cause the mechanical properties of the material to decrease. How to prepare a moisture permeable membrane material with excellent moisture permeability and excellent mechanical energy has become an urgent problem to be solved in this field. Summary of the invention

[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a polyamide-polyether block polymer composite material having both excellent moisture permeability and excellent mechanical energy.

[0005] The invention also provides a preparation method thereof, which is scientific, reasonable and suitable for large-scale production.

[0006] The invention also provides an application thereof, which can be used for preparing a water-proof and moisture-permeable membrane material.

[0007] The polyamide-polyether block polymer composite material of the present invention is prepared from the following raw materials in parts by weight: 40-80 parts of polyamide elastomer; 10-50 parts of polyolefin; 5-20 parts of functionalized polyolefin; Nanocellulose 0.1~5 parts.

[0008] The polyamide elastomer is a polymer composed of 70-90 mass parts of polyamide hard segments and 10-30 mass parts of polyether soft segments.

[0009] The polyamide hard segment is a polymer material prepared from aliphatic diamines with 6 to 12 carbon atoms and dibasic acids with 6 to 14 carbon atoms.

[0010] Preferably, the aliphatic diamine is one or more of hexamethylenediamine, decanediamine and dodecanediamine, and the dibasic acid is one or more of sebacic acid, adipic acid and dodecanediamine.

[0011] The polyether soft segment is a hydroxyl-functionalized polyether diol and an amino-functionalized polyether diamine.

[0012] Preferably, the polyether diol is one or more of polytetrahydrofuran diol, polyethylene glycol, and polypropylene glycol, and its number average molecular weight is 100-6000 g / mol, preferably 500-3000 g / mol; the polyether diamine is obtained by amination of polyether diol, preferably one or more of polyethylene oxide diamine, polytetrahydrofuran diamine, and polypropylene oxide diamine, and its number average molecular weight is 100-6000 g / mol, preferably 500-3000 g / mol.

[0013] The synthesis of the polyamide elastomer can be carried out by co-condensing a polyamide block having carboxyl groups at both ends of the chain with hydroxyl groups at both ends of the polyether chain. The preparation method of the polyamide elastomer comprises the following steps: adding aliphatic diamine, dibasic acid, polyether diamine and deionized water into a reaction container, heating to 200-230°C, maintaining a pressure of 1-1.5MPa, reacting for 1-3h, releasing the pressure to atmospheric pressure and distilling off excess water to obtain a prepolymer; adding polyether diol and a catalyst to the prepolymer, stirring evenly, evacuating and reacting at 240-280°C at a pressure of at least 1000Pa for 1-3h. Antioxidants, dyes, fillers, UV stabilizers and other additives can be added during the polymerization process.

[0014] The catalyst is a metal derivative of titanium, zirconium or hafnium, preferably tetrabutyl titanate or tetrabutyl zirconate.

[0015] The polyolefin is one or more of homopolymers or copolymers of α-olefins or dienes, including 1-butene, 1-pentene, 1-octene, 1-heptene, ethylene, propylene, etc., or combinations thereof, and the resulting polymers are LDPE, LLDPE, HDPE, PP, ethylene-propylene rubber (EPR), styrene-butadiene-styrene (SBS), etc., preferably LDPE and LLDPE.

[0016] The functionalized polyolefin is an olefin or olefin copolymer containing reactive functional groups, wherein the reactive functional groups include at least one system of epoxy, acrylic acid, glycidyl methacrylate, maleic anhydride, etc. The functionalized polyolefin is used as a solubilizer to increase the compatibility between the polyamide elastomer and the polyolefin, and the grafting rate of the functional group is 0.01% to 5% by mass, preferably between 1% and 2%.

[0017] The nanocellulose is a hydrophilic natural polymer used to improve the moisture permeability of the material.

[0018] The method for preparing the polyamide-polyether block polymer composite material of the present invention comprises the following steps: A. firstly melt-blending a polyamide elastomer and a functionalized polyolefin to obtain a mixture 1; B. After the mixture 1 is extruded into granules, the polyolefin and the nanocellulose are dry-mixed with the obtained granules, or the polyolefin, the nanocellulose and the mixture 1 are melt-blended and then extruded into granules.

[0019] The temperature of the melt blending is 140-300°C, preferably 180-220°C.

[0020] The polyamide-polyether block polymer composite material of the present invention is used for preparing water-proof and moisture-permeable membrane materials.

[0021] Compared with the prior art, the present invention has the following beneficial effects: 1) The polyamide elastomer of the present invention has a high hard segment content, and the prepared moisture-permeable film has excellent mechanical properties.

[0022] 2) The nanocellulose of the present invention has good hydrophilicity and effectively improves the moisture permeability of the moisture permeable membrane.

[0023] 3) The moisture-permeable film of the present invention has wide applicability and can be applied to the fields of textile compounding, packaging, medical treatment, etc. to meet the needs of different application scenarios. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto.

[0025] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0026] Nanocellulose: D50 diameter is 20 nm, L50 length is 2 um, and aspect ratio is 100.

[0027] Example 1 1. Synthesis of polyamide elastomer: 1900g dodecane diamine, 2615g dodecanedioic acid, 938g polytetrahydrofuran diamine with a number average molecular weight of 1000g / mol and 5000g deionized water were put into a reactor, the air in the reactor was replaced by nitrogen three times, and a polymerization reaction was started, the temperature was slowly raised to 200°C, the pressure in the reactor was kept at 1MPa for 1h, and then the pressure was slowly released to atmospheric pressure and the water in the reactor was distilled out, 938g polytetrahydrofuran diol with a number average molecular weight of 1000g / mol and 6.5g tetrabutyl zirconate were put into the reactor, the temperature was raised to 240°C and the pressure was reduced to 1000Pa for 3h, and then the material was discharged to obtain a polyamide elastomer material with a Shore hardness of 55D. The hard segment content of Example 1 is 70%.

[0028] 2. Preparation formula of polyamide elastomer and polyolefin composite material As shown in Table 1, the preparation method of the polyamide-polyether block polymer composite material comprises the following steps: A. firstly melt-blending a polyamide elastomer and a functionalized polyolefin to obtain a mixture 1; B. The polyolefin is melt-blended with the mixture 1 and then extruded into granules.

[0029] Example 2 1. Synthesis of polyamide elastomer: 2300g of decanediamine, 3000g of sebacic acid, 350g of polytetrahydrofuran diamine with a number average molecular weight of 500g / mol and 5000g of deionized water were put into a reactor, the air in the reactor was replaced by nitrogen three times, and a polymerization reaction was started, the temperature was slowly raised to 200°C, the pressure in the reactor was kept at 1MPa for 1h, and then the pressure was slowly released to atmospheric pressure and the water in the reactor was distilled out, 750g of polytetrahydrofuran diol with a number average molecular weight of 1000g / mol and 6.5g of tetrabutyl titanate were put into the reactor, the temperature was raised to 280°C and the pressure was reduced to 1000Pa for 1h, and then the material was discharged to obtain a polyamide elastomer material with a Shore hardness of 60D. The hard segment content of Example 2 is 82%.

[0030] 2. Preparation formula of polyamide elastomer and polyolefin composite material As shown in Table 1, the preparation method of the polyamide-polyether block polymer composite material comprises the following steps: A. firstly melt-blending a polyamide elastomer and a functionalized polyolefin to obtain a mixture 1; B. After the mixture 1 is extruded into pellets, the polyolefin is dry-blended with the pellets.

[0031] Example 3 1. Synthesis of polyamide elastomer: 1279g hexamethylenediamine, 2268g sebacic acid, 303g polytetrahydrofuran diamine with a number average molecular weight of 3000g / mol and 5000g deionized water were put into a reactor, the air in the reactor was replaced by nitrogen three times, and a polymerization reaction was started, the temperature was slowly raised to 200°C, the pressure in the reactor was kept at 1MPa for 1h, and then the pressure was slowly released to atmospheric pressure and the water in the reactor was distilled out, 50g polytetrahydrofuran diol with a number average molecular weight of 500g / mol and 6.5g tetrabutyl titanate were put into the reactor, the temperature was raised to 250°C and the pressure was reduced to 1000Pa for 1.5h, and then the material was discharged to obtain a polyamide elastomer material with a Shore hardness of 40D. The hard segment content of Example 3 is 90%.

[0032] 2. Preparation formula of polyamide elastomer and polyolefin composite material As shown in Table 1, the preparation method of the polyamide-polyether block polymer composite material comprises the following steps: A. firstly melt-blending a polyamide elastomer and a functionalized polyolefin to obtain a mixture 1; B. The polyolefin is melt-blended with the mixture 1 and then extruded into granules.

[0033] Table 1 Formulations of polyamide elastomer and polyolefin composite materials of Examples 1 to 3

[0034] a: The polyolefin is a commercial linear low-density polyethylene (LLDPE) having a melt index of 1.0 g / 10 min and a density of 0.918 g / cm 3 .

[0035] b: The functionalized polyolefin is a commercial ethylene-methyl methacrylate copolymer from Sumitomo Chemical of Japan with the brand name SWA330.

[0036] Examples 4, 5 and Comparative Examples 1 to 3 The method for synthesizing and preparing the polyamide elastomer material described in Example 4 is substantially the same as that in Example 3, except for the preparation formula of the polyamide elastomer and polyolefin composite material (Table 2).

[0037] The method for synthesizing and preparing the polyamide elastomer material described in Example 5 is substantially the same as that in Example 2, except for the preparation formula of the polyamide elastomer and polyolefin composite material (Table 2).

[0038] The synthesis preparation method of the polyamide elastomer material described in Comparative Example 1 is basically the same as that in Example 1, except for the preparation formula of the polyamide elastomer and the polyolefin composite material (Table 2).

[0039] The synthesis preparation method of the polyamide elastomer material described in Comparative Example 2 is basically the same as that of Example 1, except that the polymerization raw materials are: 1200 g of decanediamine, 2950 g of dodecane dicarboxylic acid, 2924 g of polytetrahydrofuran diamine with a number average molecular weight of 1000 g / mol and 2924 g of polytetrahydrofuran diol with a number average molecular weight of 1000 g / mol, and the preparation formula of the polyamide elastomer and polyolefin composite material (Table 2). The hard segment content of Comparative Example 2 is 40%.

[0040] The polyamide elastomer material synthesis preparation method and the composite material preparation formula described in Comparative Example 3 are basically the same as those in Example 5, except that all raw materials are melt-blended together during the preparation of the composite material (Table 2).

[0041] Table 2 Formulation and properties of polyamide elastomer and polyolefin composite materials of Examples 4-5 and Comparative Examples 1-3

[0042] c: The polyolefin is commercial low-density polyethylene, with a preferred melt index of 2.0 g / 10 min and a density of 0.923 g / cm 3 .

[0043] d: The functionalized polyolefin is commercial maleic anhydride grafted polyolefin (POE-g-MAH) from Mitsui Chemicals, brand POE MH5040.

[0044] The tensile strength and water vapor transmission rate tests were conducted with reference to GB / T 1040 and GB / T 1037 respectively.

[0045] Those skilled in the art will appreciate that the embodiments described herein are only intended to help readers understand the principles of the present invention, and should be understood that the protection scope of the present invention is not limited to such statements and embodiments. Those skilled in the art can make various modifications and combinations that do not deviate from the essence of the present invention based on the technical revelations disclosed by the present invention, and these modifications and combinations are still within the protection scope of the present invention.

Claims

1. A polyamide-polyether block polymer composite material, characterized in that: It is prepared from the following raw materials in parts by weight: 40-80 parts of polyamide elastomer; 10-50 parts of polyolefin; 5-20 parts of functionalized polyolefin; Nanocellulose 0.1~5 parts.

2. The polyamide-polyether block polymer composite material according to claim 1, characterized in that: The polyamide elastomer is a polymer composed of 70-90 mass parts of polyamide hard segments and 10-30 mass parts of polyether soft segments.

3. The polyamide-polyether block polymer composite material according to claim 2, characterized in that: The polyamide hard segment is a polymer prepared from an aliphatic diamine having 6 to 12 carbon atoms and a dibasic acid having 6 to 14 carbon atoms.

4. The polyamide-polyether block polymer composite material according to claim 3, characterized in that: The polyether soft segment is a hydroxyl-functionalized polyether diol and an amino-functionalized polyether diamine.

5. The polyamide-polyether block polymer composite material according to claim 4, characterized in that: The preparation method of the polyamide elastomer comprises the following steps: adding aliphatic diamine, dibasic acid, polyether diamine and deionized water into a reaction container, heating to 200-230°C, maintaining a pressure of 1-1.5MPa, reacting for 1-3h, releasing the pressure to atmospheric pressure and distilling off excess water to obtain a prepolymer; adding polyether diol and a catalyst into the prepolymer, stirring evenly, evacuating the mixture and reacting at 240-280°C under a pressure of at least 1000Pa for 1-3h.

6. The polyamide-polyether block polymer composite material according to claim 1, characterized in that: The polyolefin is one or more of homopolymers or copolymers of α-olefins or dienes.

7. The polyamide-polyether block polymer composite material according to claim 1, characterized in that: The functionalized polyolefin is an olefin or olefin copolymer containing reactive functional groups, and the reactive functional groups include epoxy, acrylic acid, glycidyl methacrylate, and maleic anhydride.

8. A method for preparing the polyamide-polyether block polymer composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: A. firstly melt-blending a polyamide elastomer and a functionalized polyolefin to obtain a mixture 1; B. After the mixture 1 is extruded into pellets, the polyolefin is dry-blended with the pellets. Alternatively, the polyolefin is melt-blended with the mixture 1 and then extruded into pellets.

9. The method for preparing the polyamide-polyether block polymer composite material according to claim 8, characterized in that: The temperature of the melt blending is 140-300°C.

10. An application of the polyamide-polyether block polymer composite material according to any one of claims 1 to 7, characterized in that: It is used to prepare water-proof and moisture-permeable membrane materials.

Citation Information

Cited By

  • Bio-based polyamide elastomer fiber as well as preparation method and application thereof