Method for preparing high-strength and high-stability wood plastic by utilizing modified high polymer granules
By preparing high-strength and high-stability wood-plastic composites from modified polymer granules, the problems of insufficient dimensional stability and mechanical properties of traditional wood-plastic composites have been solved, realizing wood-plastic composites with high strength and high thermal stability, thus expanding their application fields.
Patent Information
- Application Number
- CN202411159649.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional wood-plastic composites suffer from poor dimensional stability and unstable quality, making them difficult to apply in structural support or functional fields. Furthermore, wood powder is prone to aging and has poor mechanical properties, which limits the expansion of its application areas.
High-strength and high-stability wood-plastic composites are prepared by modifying polymer granules. Wood is treated with alkali and crushed to obtain lignofibrillated fibers, which are then melt-extruded and granulated with thermoplastic plastics and additives to form a three-dimensional mechanically interlocked structure. Combined with a stepwise extrusion feeding process, the strength and stability of the material are improved.
It significantly improves the strength and thermal stability of wood-plastic composites, with a flexural strength greater than 70 MPa, a flexural modulus exceeding 4.7 GPa, and a coefficient of thermal expansion less than 40 × 10⁻⁶/K. It solves the problems of low strength and easy thermal deformation of traditional wood-plastic composites, and improves dimensional stability and mechanical properties.
Smart Images

Figure CN118909457A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing high-strength and high-stability wood plastic, in particular to a method for preparing high-strength and high-stability wood plastic by utilizing modified polymer granules. Background Art
[0002] In the traditional wood-plastic composite material system, the utilization of wood processing residues is not sophisticated enough, and the raw materials themselves have differences in size and physical properties. The wood-plastic composite materials reinforced with wood powder still have poor dimensional stability and unstable quality. The product quality cannot be effectively guaranteed and cannot be applied to structural support or other functional fields, which seriously limits the development of products and market expansion. Therefore, exploring new processing and filling technologies for wood processing residues, studying the corresponding interface theory innovation system, and improving product quality, especially mechanical properties and stability, are the problems that urgently need to be solved to promote the high-value utilization of wood processing residues and the upgrading of wood-plastic composite materials.
[0003] At present, most wood-plastic composite materials choose to fill wood fiber powders such as wood powder and straw powder in the polymer matrix. They have problems such as easy aging and poor mechanical properties, which affects the expansion of their application areas. Summary of the invention
[0004] Purpose of the invention: The present invention aims to provide a method for preparing high-strength and high-stability wood-plastics by using modified polymer pellets. The process is simple, the use of plastic materials is reduced, the defects of traditional wood-plastics are overcome to a certain extent, and the strength and thermal stability of wood-plastics are significantly improved.
[0005] Technical solution: The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets of the present invention comprises the following steps:
[0006] The wood is subjected to alkali treatment and crushing treatment in sequence to obtain wood fiber, and the wood fiber is hydrolyzed to micro-nano level to obtain wood fiber; the wood fiber, thermoplastic plastic and additives are melt-extruded and granulated to obtain modified polymer pellets; the modified polymer pellets, wood powder and additives are then extruded, granulated and injection molded.
[0007] Furthermore, the alkali treatment and crushing treatment include: placing the wood in an alkali solution for high temperature water bath treatment for 3h to 6h, then placing it at room temperature for 12h to 24h, filtering it to neutrality and then crushing it into fibers, and the concentration of the alkali solution is 1 to 3wt%.
[0008] Furthermore, the stirring speed during the defibration is 15000-20000 rpm, and the time is 5-8 minutes.
[0009] Furthermore, the diameter of the wood broom fiber ranges from 100 nm to 100 μm.
[0010] Furthermore, the wood broom fiber is subjected to hydrophobic modification and then melt-extruded with thermoplastic plastic and additives.
[0011] Furthermore, the content of wood broom fiber in the modified polymer pellets is 10-40wt%, and the content of the auxiliary agent is 3-10wt%; the processing temperature of the extruder is 150-165°C, and the rotation speed is 20-40rpm.
[0012] Furthermore, the particle size of the wood powder ranges from 60 to 200 meshes, and the thermoplastic plastic can be recycled plastic, which is inexpensive.
[0013] Furthermore, the content of the wood fiber modified polymer granules in the modified wood plastic is 30-60wt%, the content of various additives is 3-8wt%, and the total content of the wood fiber and wood powder is 55-75wt%.
[0014] Furthermore, during the extrusion granulation, the processing temperature of the extruder is 150-170°C, and the screw speed is 15-40 rpm. The pellets after extrusion granulation are then placed in an injection molding machine for injection molding. The injection molding temperature of the injection molding machine is set to 155-170°C, and the mold temperature is 80-90°C.
[0015] Furthermore, the thermoplastic plastic includes at least one of polyethylene, polypropylene, polyvinyl chloride, nylon, polystyrene, polyester or acrylonitrile-styrene-butadiene copolymer, and the auxiliary agent includes at least one of a coupling agent or a lubricant.
[0016] The present invention can effectively improve the performance of wood-plastic composite materials by adding modified granular materials of wood fiber. Although wood fiber and wood powder are both biomass fiber materials, from a macroscopic perspective, wood powder is in powder form, while wood fiber is in silky form. Compared with wood powder, fiber can present better permeability in the composite material, play a better role in entanglement and connection, and the entanglement between flexible fibers plays an important role in improving the strength of the composite material. On the one hand, a relatively firm three-dimensional mesh mechanical interlocking structure is formed between the fiberized fiber and the plastic matrix after defibration, and the plastic matrix embeds the fiber with a certain aspect ratio therein, so the fiber plays a reinforcing role; on the other hand, the granular wood powder is further filled into the three-dimensional interlocking structure. This three-dimensional mechanical interlocking structure helps to improve the mechanical properties and dimensional stability of the modified wood-plastic. In addition, the step-by-step melt granulation process solves the problem of feeding difficulty during extrusion mixing of high-filling wood fiber, and the secondary mixing ensures the dispersibility of the wood fiber filler in the plastic matrix and enhances the mutual synergy between the fiber and the plastic matrix.
[0017] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0018] (1) Using wood fiber to modify the polymer matrix is beneficial to improve the strength and thermal stability of wood-plastic composites; fiber of the fiber grade (100nm-100μm) shows good defibrination effect and multi-scale characteristics. Single fibers are separated, and the fiber of the fiber is attached with nanofibers, which can increase the contact area with the polymer matrix, making it easier for the two to form mechanical interlocking and form a strong physical bond. The fully dispersed state of the fiber will make it play a good reinforcing role on the polymer, and at the same time it can also improve the dimensional stability of the modified wood plastic later;
[0019] (2) The problem of low strength and easy thermal deformation of traditional wood-plastic composite materials is solved; the flexural strength of the broom fiber modified wood-plastic prepared by the present invention is greater than 70MPa, the flexural modulus exceeds 4.7GPa, and the thermal expansion coefficient is less than 40×10 -6 / K, showing high strength and high dimensional stability, has huge market potential in the fields of wood-plastic building materials, furniture industry, and car body materials;
[0020] (3) A step-by-step extrusion feeding process is adopted, where wood fiber is first used to reinforce polymers, and then modified polymer pellets are extruded; the modified polymer pellets are then used to extrude and reinforce wood-plastic composites; this solves the problems of difficult feeding and difficult uniform mixing of polymer substrates and fillers in the extrusion preparation process of high-content wood fiber wood-plastic composites; reduces the appearance of bubbles and holes in the product, and improves the strength and quality stability of the product;
[0021] (4) The preparation method is simple. The wood content of up to 65-70% in the wood-plastic composite material reduces the amount of petroleum-based polymers used, which is green and environmentally friendly while reducing product costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a transmission electron micrograph of wood micro (nano) fibers after mechanical defibration;
[0023] Figure 2 This is a cross-sectional view of a 20% wood broom fiber modified polymer of Example 1;
[0024] Figure 3 This is a cross-sectional view of a polymer modified with 20% wood flour in Comparative Example 1;
[0025] Figure 4 The wood-plastic section filled with 65% wood powder in Comparative Example 2;
[0026] Figure 5 The cross-section of wood-plastic reinforced with 20% wood broom fiber modified polymer particles;
[0027] Figure 6 The bar graph of mechanical properties of modified wood plastic (a) flexural strength; (b) flexural modulus;
[0028] Figure 7 This is a bar graph of the linear thermal expansion coefficient of modified wood plastic. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0030] Example 1
[0031] The steps of preparing the high-strength and high-thermal-stability broom fiber-modified wood plastic are as follows:
[0032] (1) The raw material poplar wood shavings are placed in a 2 wt% caustic soda water bath at a high temperature of 95°C for 3 h, then placed at room temperature for 12 h, filtered to neutrality, and then crushed into fibers using a crusher;
[0033] (2) The wood fiber and the aqueous solution in step (1) are placed in a high-speed mixer at a speed of 15,000 rpm for 5 minutes to dissolve the fiber to obtain wood fiber with a diameter of 100 nm-100 μm. The fiber is mixed with γ-methacryloxypropyltrimethoxysilane at a mass ratio of 1:1 and stirred evenly, and a hydrophobic modification treatment is performed to prevent the fiber from agglomerating after dissolution;
[0034] (3) The obtained modified wood fiber, HDPE, maleic anhydride grafted polyethylene and PE wax are mixed and stirred in a ratio of 20:73:3:4, and the blend is placed in an extruder for melt extrusion molding, and after granulation, wood fiber modified HDPE pellets are obtained;
[0035] (4) The wood powder was dried and mixed with modified HDPE, maleic anhydride grafted polyethylene and PE wax in a ratio of 57:38:2:3, and then melt-mixed and extruded in an extruder to obtain modified wood-plastic pellets. The linear thermal expansion coefficient was 38.2×10 -6 / K;
[0036] (5) placing the modified wood-plastic pellets in an injection molding machine for injection molding. The injection molding temperature of the injection molding machine is set to 165°C and the mold temperature is 90°C;
[0037] Test method for the bending resistance of high-strength and high-thermal stability modified wood plastic: injection molded samples with a length of 80mm, a width of 10mm, and a thickness of 4mm were tested using a universal mechanical testing machine. The bracket span was 64mm, the pressure rod speed was 2mm / min, each sample was tested six times, and the average value of the six samples was taken.
[0038] Test method for linear thermal expansion coefficient of high-strength and high-thermal stability modified wood plastic: Take a sample of 25mm long, 4.5mm wide and 1mm thick, and test it through a static mechanical thermal analyzer (TMA), tensile mode, nitrogen atmosphere, heating rate of 5℃ / min, loading load set to 0.03N, and test each sample five times. Finally, the linear thermal expansion coefficient is calculated in the temperature range of -30℃ to 60℃, and the average value of the five sample data is taken.
[0039] The injection molded samples were subjected to flexural mechanical tests, and the results showed that the flexural strength and flexural modulus were 74.1 MPa and 4.9 GPa, respectively.
[0040] Example 2
[0041] The step (3) in Example 1 is changed to: the obtained modified wood fiber, HDPE and auxiliary agent maleic anhydride grafted polyethylene are mixed and stirred in a ratio of 10:87:3, the blend is placed in an extruder for melt extrusion molding, and wood fiber modified HDPE pellets are obtained after granulation.
[0042] The step (4) in Example 1 is changed to: drying the wood powder, mixing it with the modified HDPE, the auxiliary maleic anhydride grafted polyethylene, and the auxiliary PE wax in a ratio of 62:31:3:4, placing it in an extruder for melting and mixing, and extruding and granulating to obtain modified wood-plastic pellets; the linear thermal expansion coefficient is 40×10 -6 / K.
[0043] The remaining steps are the same as those in Example 1.
[0044] The injection molded samples were subjected to flexural mechanical tests, and the results showed that the flexural strength and flexural modulus were 72.1 MPa and 4.72 GPa, respectively.
[0045] Comparative Example 1
[0046] Unmodified wood powder, HDPE and additive maleic anhydride grafted polyethylene are mixed and stirred evenly in a ratio of 20:77:3, the blend is placed in an extruder for melt extrusion molding, and wood powder modified HDPE pellets are obtained after granulation.
[0047] Comparative Example 2
[0048] The untreated wood powder was dried and mixed with HDPE, maleic anhydride grafted polyethylene and PE wax in a ratio of 65:28:3:4. The mixture was melted and mixed in an extruder and extruded to obtain wood-plastic pellets. After injection molding, the bending strength was measured by a mechanical testing machine to be 43 MPa, and the linear thermal expansion coefficient was measured by a static thermomechanical analyzer to be 52×10 -6 / K.
[0049] like Figure 1 Shown is a transmission electron micrograph of wood micro (nano) fibers after mechanical defibration. It can be seen that the wood fibers that originally had a certain aspect ratio were effectively defibrated, and the micron-sized fiber bundles had nano-sized branches, which can be called micro-nano aggregated fibers. This type of fibers has a good defibration effect and a network structure. When subsequently mixed and extruded with a plastic matrix, the molten plastic matrix penetrates into the gaps of the fibers, and a hook-like mechanical binding force is formed between the two phases, which are interlocked and connected with each other; the fibers play a good reinforcing role.
[0050] Figure 2 This is a cross-sectional view of 20% wood fiber modified HDPE in Example 1. It can be seen that the wood fiber is evenly dispersed in the polymer matrix, the interface bonding is good, and the surface fracture is in a wire-drawing shape.
[0051] Figure 3 This is the cross section of HDPE filled with 20% wood powder in Comparative Example 1. It can be seen that the granular wood powder is aggregated into spherical accumulations. The wood powder mainly plays a filling role and has a poor reinforcing effect.
[0052] Figure 4 This is the cross section of the wood-plastic composite filled with 65% wood powder in Example 2. It can be seen that the wood powder is in the shape of islands, and the plastic is a continuous phase, forming an "island structure". The wood powder reinforcement effect is not good; this is also the reason why traditional wood-plastic composite materials are often brittle.
[0053] Figure 5 This is a cross-sectional view of the wood-plastic reinforced with 20% wood fiber modified polymer in Example 1. After adding wood powder, the content of wood fiber and wood powder in the wood-plastic composite material increases to 65%. As can be seen from the figure, the wood-plastic is mixed evenly and the interface bonding performance is good. On the one hand, a relatively strong three-dimensional mesh mechanical interlocking structure is formed between the defibrated fiber and the plastic matrix, and the plastic matrix embeds the fiber with a certain aspect ratio therein, so the fiber plays a reinforcing role; on the other hand, the granular wood powder is further filled into the three-dimensional interlocking structure. This three-dimensional mechanical interlocking structure helps to improve the mechanical properties and dimensional stability of the modified wood-plastic.
[0054] Figure 6 It is a bar graph of the mechanical properties of the two modified wood plastics obtained in Examples 1 and 2. Figure 7 The linear thermal expansion coefficient bar graph of the two modified wood plastics obtained in Examples 1 and 2 in the temperature range of -30°C to 60°C, with the unit of 10 -6 / K. Figure 6 and Figure 7In the table, "HDPE" refers to high density polyethylene, which is used as a control group; "10% PF modified wood plastic" refers to the modified polymer pellets filled with 10wt% poplar wood fiber, and the total amount of wood fiber and wood powder in the modified wood plastic reaches 65wt%, that is, Example 2; "20% PF modified wood plastic" refers to the modified polymer pellets filled with 20wt% poplar wood fiber, and the total amount of wood fiber and wood powder in the modified wood plastic reaches 65wt%, that is, Example 1.
[0055] like Figure 6 As shown in the figure, the flexural strength of wood plastic reinforced with 10% and 20% poplar fiber modified polymer pellets is greater than 70MPa and 4.7GPa. The flexural strength is about 3.5 and 5.5 times that of polyethylene HDPE, and the mechanical properties are significantly improved. Figure 7 As shown, the linear thermal expansion coefficient (CTE) of HDPE is 170×10 -6 / K; the CTE of 10% PF modified wood plastic is 40×10 -6 / K, the CTE of 20% PF modified wood plastic is 38.2×10 -6 / K is more than 3 times lower than that of HDPE, and the thermal stability and dimensional stability are greatly improved.
[0056] The present invention uses wood fiber modified polymer pellets and wood powder to mix and knead to prepare a high-strength and high-stability wood-plastic composite material, and the step-by-step granulation extrusion optimizes the process. The prepared modified wood-plastic has a high wood content, which reduces the consumption of petroleum-based polymers. Recycled HDPE can be used in the embodiment to promote the recycling of resources. The obtained product has excellent mechanical and thermal properties, and it can be considered to select a polymer substrate with better performance or add a coupling agent, stabilizer, reinforcing agent, etc. to obtain further improvement in performance.
Claims
1. A method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets, characterized in that: The steps include: The wood is sequentially subjected to alkali treatment and crushing treatment to obtain wood fiber, and the wood fiber is hydrolyzed to micro-nano level to obtain wood fiber; the wood fiber, thermoplastic plastic and additives are then melt-extruded and granulated to obtain modified polymer pellets; The modified polymer pellets, wood powder and additives are then extruded into pellets and injection molded.
2. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The alkali treatment and crushing treatment comprises: placing the wood in a 1-3wt% alkali solution for water bath treatment for 3h-6h, then placing it at room temperature for 12h-24h, washing and filtering to neutrality, and then crushing it into fibers.
3. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The stirring speed during the defibration is 15000-20000 rpm, and the time is 5-8 minutes.
4. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The diameter of the wood broom fiber ranges from 100 nm to 100 μm.
5. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The processing temperature of the melt extrusion is 150-165° C., and the rotation speed is 20-40 rpm.
6. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The content of wood broom fiber in the modified polymer granules is 10-40wt%, and the content of the auxiliary agent is 3-10wt%.
7. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The particle size of the wood powder ranges from 60 to 200 meshes.
8. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The content of modified polymer particles in the modified wood plastic is 30-60wt%, the content of various additives is 3-8wt%, and the total content of wood broom fiber and wood powder is 55-75wt%.
9. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: During the extrusion granulation, the processing temperature of the extruder is 150-170°C, the screw speed is 15-40rpm, and during the injection molding, the injection temperature of the injection molding machine is set to 155-170°C, and the mold temperature is 80-90°C.
10. The method for preparing high-strength and high-stability wood-plastic by using modified polymer pellets according to claim 1, characterized in that: The thermoplastic comprises at least one of polyethylene, polypropylene, polyvinyl chloride, nylon, polystyrene, polyester or acrylonitrile-styrene-butadiene copolymer, and the auxiliary agent comprises at least one of a coupling agent or a lubricant.
Citation Information
Cited By
Method for optimizing mechanical property of bio-based composite material based on nano modification
CN120727172A