Gel pen ink with optimized writing performance and preparation method thereof
The stability and intermittent writing performance of neutral pen ink were solved by using modified active red 120 dye and nanocellulose grafting, three-dimensional network structure of chitosan and glycine in neutral pen ink, and combinations of other modifiers. The poor problem has achieved significant improvement in the dryness resistance and writing performance of the ink, meeting the demand of the high-end market.
Patent Information
- Application Number
- CN202410915917.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-08
AI Technical Summary
The existing neutral pen ink has problems such as poor stability and poor intermittent writing performance, resulting in poor writing.
Using modified active red 120 dye, pectin, thickener, dispersant, modifier, antibacterial and anti-mold agent, surfactant and antifreeze agent, etc., the modified active red 120 dye, shell is modified by nanocellulose grafting. Glycan and glycine form a three-dimensional network structure, chemical bonds of 3-(methylamine)-1-propanol and 4-amino-1-butanol, synergistic effects of ethyl palmitate, nanosilica and sugar alcohol to enhance ink dispersibility, stability and liquidity.
It realizes the dry resistance of ink, intermittent writing fluency, long shelf life and stability, ensuring the improvement of writing performance and meeting the demand of high-end market.
Smart Images

Figure BDA0004935088350000081 
Figure BDA0004935088350000091 
Figure BDA0004935088350000092
Abstract
Description
Technical Field
[0001] This application relates to the field of inks, and more particularly to a neutral pen ink with optimized writing performance and a method for preparing the same. Background Technology
[0002] Neutral ink ballpoint pens (hereinafter referred to as neutral pens) overcome the shortcomings of oil-based ballpoint pens, such as uneven writing and difficulty in writing, and water-based ballpoint pens, which bleed through the paper. Furthermore, due to their advantages such as smooth writing, full ink coverage, and quick drying, they have been favored by consumers since their introduction. In recent years, research on neutral inks designed to complement neutral pens has been increasing.
[0003] Good writing smoothness is an important indicator of high-quality neutral ink. High-quality neutral ink can significantly reduce pen tip wear during writing, while providing the writer with a comfortable writing experience. The addition of surfactants to neutral ink helps disperse pigment particles in the system, preventing them from agglomerating, flocculating, and settling; it also helps the ink detach from the writing instrument surface and spread on the writing surface; and it improves the lubricity of the neutral ink, resulting in a smooth writing experience and even, full lines. Currently, neutral pen inks suffer from poor stability and intermittent writing performance, leading to uneven writing. Summary of the Invention
[0004] The purpose of this application is to address the shortcomings of current technologies by providing a neutral pen ink with optimized writing performance and its preparation method. The neutral pen ink with optimized writing performance prepared in this application has advantages such as good ink drying resistance, smooth intermittent writing, long ink shelf life, and good stability in use, meeting the demands of the high-end market.
[0005] In a first aspect, this application provides a neutral pen ink with optimized writing performance, employing the following technical solution: A neutral pen ink with optimized writing performance comprises, by weight, the following raw materials: 5.8-6.2 parts modified reactive red 120 dye, 1.5-1.8 parts pectin, 1.2-1.5 parts thickener, 5.6-6.2 parts dispersant, 2-2.5 parts modifier, 0.1-0.2 parts antibacterial and antifungal agent, 1-3 parts surfactant, 1-2 parts antifreeze, and 35-39 parts deionized water.
[0006] By adopting the above technical solutions, the writing performance optimized gel pen ink of this application achieves advantages such as good ink drying resistance, smooth intermittent writing, long ink shelf life, and good usage stability through the synergistic effect of each component. Modified Reactive Red 120 dye: Nanocellulose grafted onto modified Reactive Red 120 dye enhances the dispersibility and compatibility of Reactive Red 120 dye in the gel pen ink system, thereby reducing the system's flow resistance, improving the ink's writing smoothness, and thus significantly improving the stability and writing performance of the gel pen ink. Pectin: Soluble in water but insoluble in alcohol, it improves the stability of the ink system; and after writing, pectin combines with Ca and Mg in the paper to form a gel, thereby achieving rapid fixation of the writing. Thickener: Utilizing the easy formation of an elastic three-dimensional network structure by chitosan and glycine in the ink system, a thickening effect is achieved; at the same time, the water-insoluble property of chitosan helps to achieve long-term stability of the gel pen ink dispersion system. Furthermore, after the ink is applied to paper, as the water evaporates, chitosan and glycine form a friction-resistant film, protecting the writing from damage and destruction caused by external forces. Dispersant: Prevents pigment particle aggregation, ensuring stable dispersion of modified Reactive Red 120 dye particles in the neutral ink system. The increased adsorption of modified Reactive Red 120 dye particles by the dispersant reduces the probability of particle aggregation, increasing the sliding force between the dye particles and reducing the internal friction between particles and between particles and the solvent, thereby reducing the flow resistance of the system and improving the writing smoothness of the ink. Modifier: Improves the ink's drying resistance, intermittent writing performance, and stability during use. Antibacterial and antifungal agents: Prevent mold and bacterial growth during ink use, ensuring ink quality and safety. Surface activator: Effectively controls the surface tension of the ballpoint pen ink to be close to that of the writing paper, thus effectively reducing ink buildup and uneven color caused by excessive diffusion after writing; at the same time, it further stabilizes the color of the writing, without obvious differences in light and dark shades. Antifreeze: Prevents the ink from freezing in low-temperature environments, ensuring normal ink flow and use. Deionized water: As a solvent, it ensures good dissolution and dispersion of the various components in the ink.
[0007] Preferably, the preparation method of the modified Reactive Red 120 dye includes the following steps: S21. According to the mass fraction, add 10 parts of nanocellulose, 300 parts of Reactive Red 120 dye, 20 parts of sodium carbonate and 100 parts of deionized water to the reactor in sequence, stir evenly, then heat to 80-82℃, keep the temperature for 90-95 minutes, cool to room temperature to obtain reaction solution A. S22. According to the mass fraction, transfer reaction solution A to a container, add 4000 parts of deionized water, stir evenly, and centrifuge at 6000 rpm. The obtained modified reactive red 120 dye precipitate is redispersed in 4000 parts of deionized water, and 40 parts of ammonium bicarbonate is added and stirred evenly. Centrifuge at 6000 rpm and retain the modified reactive red 120 dye precipitate. Repeat this step until the supernatant after centrifugation becomes colorless and all unreacted reactive red 120 dye is removed. Disperse the final modified reactive red 120 dye precipitate in 300 parts of deionized water and perform vacuum distillation on it at 55℃ and -0.1MPa using a rotary evaporator to decompose the residual ammonium bicarbonate into ammonia and carbon dioxide, which are then removed from the modified reactive red 120 dye suspension. Finally, pure nanocellulose grafted modified reactive red 120 dye is obtained and stored in a refrigerator at 4℃ for later use.
[0008] By adopting the above technical solution, the Reactive Red 120 dye is grafted and modified with nanocellulose to obtain high-purity nanocellulose grafted and modified Reactive Red 120 dye. This improves the dispersibility and compatibility of Reactive Red 120 dye in the gel pen ink system, reduces the flow resistance of the system, and improves the writing lubrication of the ink, thereby significantly improving the stability and writing performance of the gel pen ink.
[0009] Preferably, the thickener is composed of chitosan and glycine in a mass ratio of 3:2.
[0010] By employing the above technical solution, chitosan easily forms a flexible three-dimensional network structure in the ink system. This structure effectively increases the viscosity of the ink, thus achieving a thickening effect. Glycine also participates in the formation of this three-dimensional network structure, working together with chitosan to make the ink system more stable. The ink flow during writing is controlled, preventing the ink from becoming too thin and causing blurred or bleed-through writing. Chitosan helps achieve long-term stability of the ballpoint pen ink dispersion system. As a small-molecule amino acid, glycine can fill the network structure formed by chitosan, enhancing the network's density and stability, thereby further improving the ink's storage and usage stability. After the ink is written on paper, as the water evaporates, chitosan and glycine form an abrasion-resistant film. This film not only protects the written text from damage and destruction caused by external forces but also prevents the text from becoming blurred or fading due to friction. The combination of chitosan and glycine, through the formation of a stable three-dimensional network structure, not only achieves the ink thickening effect but also improves the ink's stability and the abrasion resistance of the written text. The synergistic effect between the two further enhances the overall performance of the ink, meeting the high-end market's demand for writing performance.
[0011] Preferably, the dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a mass ratio of 3:5.
[0012] By employing the above technical solution, 3-(methylamino)-1-propanol and 4-amino-1-butanol, as dispersants, can form chemical bonds with the N and OH groups on the surface of the modified Reactive Red 120 dye particles. This chemical bond formation improves the dispersion stability of the dye particles in the ink system, prevents aggregation between pigment particles, and thus makes the ink color more uniform during writing, reducing the formation of stains and sediment. Through chemical bonding with the surface groups of the dye particles, 3-(methylamino)-1-propanol and 4-amino-1-butanol also enhance the ink's resistance to bleeding. This means that the ink diffusion on the paper is effectively controlled, the color density and edge clarity of the writing are improved, making the writing clearer and more durable. The combination of 3-(methylamino)-1-propanol and 4-amino-1-butanol, through the interaction of their respective functional groups with the dye particles, achieves a better dispersion effect than a single component. The molecular structure of 3-(methylamino)-1-propanol provides strong polarity, which helps to form a more stable adsorption layer with dye particles; while 4-amino-1-butanol provides steric hindrance through its long carbon chain, further preventing particle aggregation. This synergistic effect ensures the long-term stable dispersion of pigment particles in the ink, avoiding writing problems caused by aggregation. In summary, the dispersant composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a 3:5 mass ratio plays a role in dispersing stability, improving bleed resistance, and synergistic enhancement in the gel pen ink of this application. These effects collectively improve the writing performance of the ink, meeting the demands of the high-end market for writing performance.
[0013] Preferably, the modifier is composed of ethyl palmitate, nano-silica, and sugar alcohol in a mass ratio of 3:3:2.
[0014] By employing the above technical solutions, ethyl palmitate plays a moisturizing and lubricating role in the ink, helping to prevent ink from flowing in high humidity environments and drying at the pen tip, thereby improving the ink's resistance to drying and intermittent writing performance. This means that even after prolonged periods of non-use, the ink can still write smoothly without easily running dry or drying out. After writing, ethyl palmitate quickly forms a protective film, enhancing the gloss of the writing and making the characters brighter and more vivid. This property is particularly suitable for writing occasions that emphasize visual effects, such as artistic creation or high-end business documents. Nano-silica forms a three-dimensional network structure in the ink through electrostatic interactions, providing elastic components and improving the ink's rheological properties. This structure helps the ink form a stable film at the pen tip, preventing leakage, and simultaneously allows for rapid recovery of fluidity during writing, reducing writing resistance. Sugar alcohols, as part of the modifier, have excellent moisturizing properties, further preventing ink from flowing in high humidity environments and improving the ink's resistance to drying. Sugar alcohols also help maintain the stability of the ink system, reducing stratification and sedimentation caused by temperature changes or long-term storage. The combination of ethyl palmitate, nano-silica, and sugar alcohol complements each other's properties, achieving a comprehensive improvement in ink performance. Ethyl palmitate and sugar alcohol work together to enhance the ink's drying resistance and moisture retention; nano-silica, by forming a three-dimensional network structure, enhances the ink's rheological properties and writing smoothness. This synergistic effect ensures the ink exhibits excellent writing performance under various environmental conditions, meeting the demands of the high-end market. In summary, the modifier composed of ethyl palmitate, nano-silica, and sugar alcohol in a 3:3:2 mass ratio plays a multiple role in the neutral pen ink of this application, including improving drying resistance, enhancing writing gloss, forming a three-dimensional network structure, and enhancing writing smoothness. These effects collectively improve the ink's overall writing performance, meeting the needs of the high-end market.
[0015] Preferably, the average particle size of the nano-silica is 50 nanometers.
[0016] Preferably, the antibacterial and antifungal agent is one of benzotriazole and dithiocarbamate.
[0017] Preferably, the surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether, and tetradecyl dimethylamine oxide in a mass ratio of 4:3:2-3.
[0018] By employing the above technical solution, the main function of the surfactant is to adjust the surface tension of the ballpoint pen ink, making it closer to the surface tension of the writing paper. Oil-based polyoxyethylene glycol ether and high-carbon fatty alcohol polyoxyethylene ether, as nonionic surfactants, can form an ordered molecular layer at the ink-paper interface, thereby reducing surface tension and improving the ink's spreadability on the paper, reducing accumulation and diffusion during writing. Tetradecyl dimethylamine oxide, as a cationic surfactant, has a positive charge that can interact with negatively charged particles in the ink, enhancing the stability of the ink system. Simultaneously, its long-chain alkyl groups can form hydrophobic interactions with the long-chain alkyl groups of the oil-based polyoxyethylene glycol ether and high-carbon fatty alcohol polyoxyethylene ether, further stabilizing the surfactant molecular layer in the ink. This mixture of three surfactants, while reducing the surface tension of the ink, also reduces friction at the pen tip, improving writing smoothness. This lubrication effect is due to the lubricating film formed by the surfactant molecules on the ink-pen tip contact surface, reducing writing resistance and making the writing process smoother. Because surfactants effectively control ink behavior on paper, they also help improve the uniformity of handwriting. Oil-based polyoxyethylene glycol ethers and high-carbon fatty alcohol polyoxyethylene ethers adjust the ink's spreadability, resulting in more uniform handwriting during drying and reducing color differences caused by inconsistent ink flow. The combination of oil-based polyoxyethylene glycol ethers, high-carbon fatty alcohol polyoxyethylene ethers, and tetradecyl dimethylamine oxide complements each other through their respective properties, achieving a comprehensive improvement in ink performance. The combination of nonionic and cationic surfactants not only optimizes the ink's surface tension but also enhances the stability of the ink system and the smoothness during writing. This synergistic effect ensures that the ink exhibits excellent writing performance under various environmental conditions, meeting the demands of the high-end market.
[0019] Preferably, the antifreeze is at least one of ethylene glycol and diethylene glycol.
[0020] Secondly, this application provides a method for preparing neutral pen ink with optimized writing performance, employing the following technical solution: As a general technical concept, this application also provides a method for preparing the above-mentioned writing performance optimized neutral pen ink, including the following steps: S101. According to the mass fractions, place pectin, thickener, dispersant, modifier, antibacterial and antifungal agent, surfactant, antifreeze and deionized water in a container and stir. Heat to 55℃ and sonicate for 50-60 minutes to obtain mixture A. S102. Add the modified reactive red 120 dye to the mixture A according to the mass fraction. Stir at room temperature for 2-3 hours and then perform vacuum degassing to obtain neutral pen ink with optimized writing performance.
[0021] In summary, the beneficial technical effects of this application are as follows: 1. Good ink drying resistance: The use of modified Reactive Red 120 dye and pectin and other raw materials improves the stability of the ink in dry environments and reduces writing problems caused by ink drying.
[0022] 2. Smooth intermittent writing: By adding dispersants and surfactants, the ink's fluidity and stability are improved, allowing pen tips that have not been used for a long time to quickly regain their writing ability.
[0023] 3. Long ink shelf life: The use of antibacterial and antifungal agents and thickeners extends the ink's lifespan and reduces the risk of ink deterioration.
[0024] 4. Good stability: By adding modifiers and nano-silica, the stability of the ink in different environments is improved, making the writing effect more stable and reliable.
[0025] 5. Quick fixation of writing: Pectin combines with Ca and Mg in the paper to form a gel, which allows the writing to be quickly fixed on the paper, improving writing efficiency.
[0026] 6. Uniform ink color: The dispersant and surfactant make the ink spread more evenly on the paper, avoiding the problem of uneven ink color. Detailed Implementation
[0027] The embodiments and preparation examples of this application will be described in detail below. However, those skilled in the art will understand that the following embodiments and preparation examples are for illustrative purposes only and should not be considered as limiting the scope of this application. Unless otherwise specified in the embodiments and preparation examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available products. Reactive Red 120 dye was purchased from Sigma-Aldrich China.
[0028] Preparation Example 1: Preparation of Modified Reactive Red 120 Dye The preparation method of modified reactive red 120 dye includes the following steps: S21. According to the mass fraction, add 10g of nanocellulose, 300g of Reactive Red 120 dye, 20g of sodium carbonate and 100g of deionized water to the reactor in sequence, stir evenly, then heat to 80-82℃, keep the temperature for 93 minutes, cool to room temperature to obtain reaction solution A. S22. According to the mass fraction, transfer reaction solution A to a container, add 4000g of deionized water, stir evenly, and centrifuge at 6000 rpm. The obtained modified reactive red 120 dye precipitate is redispersed in 4000g of deionized water, 40g of ammonium bicarbonate is added and stirred evenly, and centrifuged at 6000 rpm, retaining the modified reactive red 120 dye precipitate; repeat this step until the supernatant after centrifugation becomes colorless and all unreacted reactive red 120 dye is removed. Disperse the final modified reactive red 120 dye precipitate in 300g of deionized water, and perform vacuum distillation on it using a rotary evaporator at 55℃ and -0.1MPa to decompose the residual ammonium bicarbonate into ammonia and carbon dioxide and remove them from the modified reactive red 120 dye suspension, finally obtaining pure nanocellulose grafted modified reactive red 120 dye, which is stored in a refrigerator at 4℃ for later use.
[0029] Example 1 A neutral pen ink with optimized writing performance comprises, by weight parts, the following raw materials: 5.8g modified reactive red 120 dye, 1.5g pectin, 1.2g thickener, 5.6g dispersant, 2g modifier, 0.1g benzotriazole, 1g surfactant, 1g ethylene glycol, and 35g deionized water. The thickener is composed of chitosan and glycine in a weight ratio of 3:2. The dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a weight ratio of 3:5. The modifier is composed of ethyl palmitate, nano-silica (average particle size of 50 nm), and sugar alcohol in a weight ratio of 3:3:2. The surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether, and tetradecyl dimethylamine oxide in a weight ratio of 4:3:2.
[0030] The above-mentioned method for preparing a neutral pen ink with optimized writing performance includes the following steps: S101. According to the mass fractions, pectin, thickener, dispersant, modifier, benzotriazole, surfactant, ethylene glycol and deionized water are placed in a container and stirred. The mixture is heated to 55°C and ultrasonically treated for 50 minutes to obtain mixture A. S102. Add the modified reactive red 120 dye to the mixture A according to the mass fraction. Stir at room temperature for 2 hours and then perform vacuum degassing to obtain neutral pen ink with optimized writing performance.
[0031] Example 2 A neutral pen ink with optimized writing performance comprises, by weight parts, the following raw materials: 6.2g modified reactive red 120 dye, 1.8g pectin, 1.5g thickener, 6.2g dispersant, 2.5g modifier, 0.2g dithiocarbamate, 3g surfactant, 2g diethylene glycol, and 39g deionized water. The thickener is composed of chitosan and glycine in a weight ratio of 3:2. The dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a weight ratio of 3:5. The modifier is composed of ethyl palmitate, nano-silica (average particle size of 50 nm), and sugar alcohol in a weight ratio of 3:3:2. The surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether, and tetradecyl dimethylamine oxide in a weight ratio of 4:3:3.
[0032] The above-mentioned method for preparing a neutral pen ink with optimized writing performance includes the following steps: S101. According to the mass fractions, pectin, thickener, dispersant, modifier, dithiocarbamate, surfactant, diethylene glycol and deionized water are placed in a container and stirred. The mixture is heated to 55°C and ultrasonically treated for 60 minutes to obtain mixture A. S102. Add the modified reactive red 120 dye to the mixture A according to the mass fraction. Stir at room temperature for 3 hours and then perform vacuum degassing to obtain neutral pen ink with optimized writing performance.
[0033] Example 3 A neutral pen ink with optimized writing performance comprises, by weight parts, the following raw materials: 6g modified reactive red 120 dye, 1.7g pectin, 1.3g thickener, 6g dispersant, 2.3g modifier, 0.15g benzotriazole, 2g surfactant, 1.5g ethylene glycol, and 37g deionized water. The thickener is composed of chitosan and glycine in a weight ratio of 3:2. The dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a weight ratio of 3:5. The modifier is composed of ethyl palmitate, nano-silica (average particle size of 50 nm), and sugar alcohol in a weight ratio of 3:3:2. The surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether, and tetradecyl dimethylamine oxide in a weight ratio of 4:3:2.5.
[0034] The above-mentioned method for preparing a neutral pen ink with optimized writing performance includes the following steps: S101. According to the mass fractions, pectin, thickener, dispersant, modifier, benzotriazole, surfactant, ethylene glycol and deionized water are placed in a container and stirred. The mixture is heated to 55°C and ultrasonically treated for 55 minutes to obtain mixture A. S102. According to the mass fraction, add the modified reactive red 120 dye to the mixture A, stir at room temperature for 2.6 hours, and then perform vacuum degassing to obtain the neutral pen ink with optimized writing performance.
[0035] Comparative Example 1 Similar to Example 3, except that the thickener is chitosan.
[0036] Comparative Example 2 Same as in Example 3, except that the thickener is glycine.
[0037] Comparative Example 3 Same as in Example 3, except that the dispersant is 3-(methylamino)-1-propanol.
[0038] Comparative Example 4 Same as in Example 3, except that the dispersant is 4-amino-1-butanol.
[0039] Comparative Example 5 Same as in Example 3, except that the modifier is ethyl palmitate.
[0040] Comparative Example 6 Similar to Example 3, except that the modifier is nano-silica (average particle size of 50 nanometers).
[0041] Comparative Example 7 Similar to Example 3, except that the modifier is a sugar alcohol.
[0042] Comparative Example 8 Similar to Example 3, except that the surfactant is an oil-based polyoxyethylene glycol ether.
[0043] Comparative Example 9 Similar to Example 3, except that the surfactant is a high-carbon fatty alcohol polyoxyethylene ether.
[0044] Comparative Example 10 Same as in Example 3, except that the surfactant is tetradecyl dimethylamine oxide.
[0045] Comparative Example 11 Similar to Example 3, except that an equal amount of Reactive Red 120 dye was used instead of the modified Reactive Red 120 dye.
[0046] Performance testing Using a writing and drawing machine (model BLD-8032) manufactured by Dongguan Bolade Co., Ltd., and 80g engineering drawing paper from Jinfeng Paper Industry, the writing performance of the neutral pen inks prepared in Examples 1-3 and Comparative Examples 1-11 was tested according to the specific requirements of "QB / T 2625-2011 Neutral Ink Ballpoint Pens and Refills" and the pen tip (ball diameter D: 0.55mm≤D<0.75mm) with "pen tip classification: fine, pen tip code: F" as specified in "QB / T2625-2011 Neutral Ink Ballpoint Pens and Refills". The writing performance of the neutral pen inks is shown in Table 1, the intermittent writing performance of the neutral pen inks is shown in Table 2, and the preservation performance of the neutral pen inks is shown in Table 3.
[0047] Table 1. Writing performance of gel pen ink Table 2 Intermittent writing performance of gel pen ink project Intermittent writing performance Example 1 After a 24-hour interval, writing is normal within 500mm, and the lines are of uniform thickness. Example 2 After a 24-hour interval, writing is normal within 500mm, and the lines are of uniform thickness. Example 3 After a 24-hour interval, writing is normal within 500mm, and the lines are of uniform thickness. Comparative Example 1 After a 24-hour interval, writing is normal within 500mm, and the lines are of uniform thickness. Comparative Example 2 After a 24-hour interval, writing is normal within 500mm, and the lines are of uniform thickness. Comparative Example 3 After a 24-hour interval, writing is normal within 400mm, and the lines are of uniform thickness. Comparative Example 4 After a 24-hour interval, writing is normal within 400mm, and the lines are of uniform thickness. Comparative Example 5 After a 24-hour interval, writing is normal within 300mm, and the lines are of uniform thickness. Comparative Example 6 After a 24-hour interval, writing is normal within 300mm, and the lines are of uniform thickness. Comparative Example 7 After a 24-hour interval, writing is normal within 300mm, and the lines are of uniform thickness. Comparative Example 8 After a 24-hour interval, writing is normal within 350mm, and the lines are of uniform thickness. Comparative Example 9 After a 24-hour interval, writing is normal within 350mm, and the lines are of uniform thickness. Comparative Example 10 After a 24-hour interval, writing is normal within 350mm, and the lines are of uniform thickness. Comparative Example 11 After a 24-hour interval, writing within 120mm is normal, and the lines are of uniform thickness. Table 3. Preservation properties of ballpoint pen ink Analyzing the data in Tables 1, 2, and 3, we can see that: 1) The neutral pen inks with optimized writing performance prepared in Examples 1-3 have advantages such as good ink drying resistance, smooth intermittent writing, long ink shelf life, and good usage stability. The writing performance far exceeds the requirements of "QB / T 2625-2011 Neutral Ink Ballpoint Pens and Refills"; the intermittent writing performance far exceeds the requirements of "QB / T 2625-2011 Neutral Ink Ballpoint Pens and Refills"; the shelf life far exceeds the requirements of "QB / T 2625-2011 Neutral Ink Ballpoint Pens and Refills"; and it meets the needs of the high-end market.
[0048] 2) The performance comparison analysis of the writing performance optimized neutral pen inks prepared in Example 3 and Comparative Examples 1-2 shows that the thickener is composed of chitosan and glycine in a mass ratio of 3:2. By utilizing their synergistic effect, a stable three-dimensional network structure is formed, which not only achieves the thickening effect of the ink, but also improves the stability of the ink and the abrasion resistance of the writing, further enhancing the overall performance of the ink and meeting the demand for writing performance in the high-end market.
[0049] 3) A comparative analysis of the writing performance of the neutral pen inks with optimized writing properties prepared in Example 3 and Comparative Examples 3-4 shows that the dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a mass ratio of 3:5. As dispersants, the N and OH groups of 3-(methylamino)-1-propanol and 4-amino-1-butanol can form chemical bonds with the groups on the surface of the modified Reactive Red 120 dye particles. This chemical bond formation improves the dispersion stability of the dye particles in the ink system, prevents aggregation between pigment particles, and thus makes the ink color more uniform during writing, reducing the formation of stains and sediment. Their synergistic effect ensures the long-term stable dispersion of pigment particles in the ink, avoiding writing problems caused by aggregation.
[0050] 4) A comparative analysis of the performance of the optimized gel pen inks prepared in Example 3 and Comparative Examples 5-7 shows that the modifier, composed of ethyl palmitate, nano-silica, and sugar alcohol in a mass ratio of 3:3:2, utilizes the synergistic effect between ethyl palmitate, nano-silica, and sugar alcohol to achieve a comprehensive improvement in ink performance through their complementary properties. Ethyl palmitate and sugar alcohol work together to improve the ink's drying resistance and moisture retention; nano-silica, by forming a three-dimensional network structure, enhances the ink's rheological properties and writing smoothness. This synergistic effect ensures that the ink exhibits excellent writing performance under different environmental conditions, meeting the demands of the high-end market for writing performance.
[0051] 5) A comparative analysis of the writing performance of the gel pen inks prepared in Example 3 and Comparative Examples 8-10 shows that the surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether, and tetradecyl dimethylamine oxide in a mass ratio of 4:3:2.5. Utilizing the synergistic effect among these components, the ink's performance is comprehensively improved through their complementary properties. The combination of nonionic and cationic surfactants not only optimizes the surface tension of the ink but also enhances the stability of the ink system and the lubricity during writing. This synergistic effect ensures that the ink exhibits excellent writing performance under various environmental conditions, meeting the demands of the high-end market.
[0052] 6) The performance comparison analysis of the writing performance optimized neutral pen inks prepared in Example 3 and Comparative Example 11 shows that grafting Reactive Red 120 dye with nanocellulose to obtain high-purity nanocellulose grafted modified Reactive Red 120 dye significantly improves the dispersibility and compatibility of Reactive Red 120 dye in the neutral pen ink system, reduces the flow resistance of the system, and improves the writing lubrication of the ink, thereby significantly improving the stability and writing performance of the neutral pen ink.
[0053] The above embodiments are only used to explain the technical solutions of this application and are not intended to limit it. Although the above embodiments have provided specific descriptions of this application, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation methods of this application. Any modifications and equivalent substitutions that do not depart from the spirit and scope of this application should be covered within the protection scope of this application.
Claims
1. A gel pen ink with optimized writing performance, characterized in that: The preparation raw materials include the following by weight: 5.8-6.2 parts of modified reactive red 120 dye, 1.5-1.8 parts of pectin, 1.2-1.5 parts of thickener, 5.6-6.2 parts of dispersant, 2-2.5 parts of modifier, 0.1-0.2 parts of antibacterial and mildewproof agent, 1-3 parts of surfactant, 1-2 parts of antifreeze agent and 35-39 parts of deionized water.
2. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The preparation method of the modified reactive red 120 dye comprises the following steps: S21, according to the mass fraction, in the reactor, add 10 parts of nanocellulose, 300 parts of reactive red 120 dye, 20 parts of sodium carbonate and 100 parts of deionized water in sequence, stir evenly, then heat to 80-82°C, keep warm for 90-95 minutes, cool to room temperature, and obtain reaction solution A; S22. According to the mass fraction, the reaction solution A is transferred to a container, 4000 parts of deionized water is added, and after stirring, the mixture is centrifuged at a speed of 6000 rpm to obtain a modified reactive red 120 dye precipitate, which is redispersed in 4000 parts of deionized water, and 40 parts of ammonium bicarbonate are added to stir and mix evenly, and the mixture is centrifuged at a speed of 6000 rpm to retain the modified reactive red 120 dye precipitate; this step is repeated until the supernatant after centrifugation becomes colorless and all unreacted reactive red 120 dye is removed, and the modified reactive red 120 dye precipitate finally obtained is dispersed in 300 parts of deionized water, and is subjected to reduced pressure distillation at 55° C. and -0.1 MPa using a rotary evaporator to decompose the residual ammonium bicarbonate into ammonia and carbon dioxide, which are removed from the modified reactive red 120 dye suspension, and finally a pure nanocellulose grafted modified reactive red 120 dye is obtained, which is placed in a 4° C. refrigerator for standby use.
3. The gel pen ink with optimized writing performance according to claim 1, characterized in that: The thickener is composed of chitosan and glycine in a mass ratio of 3:
2.
4. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The dispersant is composed of 3-(methylamino)-1-propanol and 4-amino-1-butanol in a mass ratio of 3:
5.
5. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The modifier consists of ethyl palmitate, nano silicon dioxide and sugar alcohol in a mass ratio of 3:3:
2.
6. A gel pen ink with optimized writing performance according to claim 5, characterized in that: The average particle size of the nano silicon dioxide is 50 nanometers.
7. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The antibacterial and mildew-proof agent is one of benzotriazole and dithiocarbamate.
8. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The surfactant is composed of oil-based polyoxyethylene glycol ether, high-carbon fatty alcohol polyoxyethylene ether and tetradecyl dimethyl amine oxide in a mass ratio of 4:3:2-3.
9. A gel pen ink with optimized writing performance according to claim 1, characterized in that: The antifreeze agent is at least one of ethylene glycol and diethylene glycol.
10. A method for preparing a gel pen ink with optimized writing performance as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: S101, according to the mass fractions, pectin, thickener, dispersant, modifier, antibacterial and antifungal agent, surfactant, antifreeze agent and deionized water are placed in a container, stirred, heated to 55° C., and ultrasonically treated for 50-60 min to obtain a mixed solution A; S102. Add modified reactive red 120 dye to mixed solution A according to the mass fraction, stir at room temperature for 2-3 hours, and then perform vacuum degassing to obtain gel pen ink with optimized writing performance.