Self-polishing antifouling paint and preparation method thereof

By esterification reaction of capsaicin and acrylic resin, capsaicin-modified acrylic resin was prepared as a matrix, and combined with other components, the problem of strong irritation in the production process is solved, achieving efficient anti-fouling Improve performance and safety to meet the pollution prevention needs of marine equipment.

CN118909499AActive Publication Date: 2024-11-08HUBEI INST OF AEROSPACE CHEMOTECHNOLOGY

Patent Information

Application Number
CN202411165370.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing capsaicin anti-fouling paint is highly irritating due to capsaicin volatilization during production and construction, which affects the safety of staff. The commonly used zinc acrylate and silicon acrylate self-polishing resins lack anti-fouling properties.

Method used

Capsaicin modified acrylic resin is used as the matrix resin, and capsaicin and acrylic prepolymer are grafted through esterification reaction to reduce the irritation of capsaicin and improve the antifouling performance, and combine rosin, paraffin chloride, cuprous oxide, Zinc oxide, copper pyrithione, talc powder, iron oxide red and dispersant, prepare anti-fouling paint with self-polishing and anti-fouling properties.

Benefits of technology

It significantly reduces the irritation of capsaicin, improves the anti-fouling ability and physical properties of anti-fouling paint, meets the anti-fouling needs of marine equipment, and improves the safety and effect of the product by reducing the use of copper oxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909499A_ABST
    Figure CN118909499A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of marine coatings, and particularly discloses a self-polishing antifouling paint and a preparation method thereof, and the self-polishing antifouling paint comprises the following components in parts by weight: 100 parts of capsaicin modified acrylic resin; 40 to 50 parts of rosin; 10 to 25 parts of chlorinated paraffin; 25 to 30 parts of xylene; 110 to 150 parts of cuprous oxide; 35-50 parts of zinc oxide; 17 to 35 parts of copper pyrithione; 10 to 20 parts of talcum powder; 15-30 parts of iron oxide red; and 10-15 parts of a dispersant. The self-polishing antifouling paint adopts the capsaicin modified acrylic resin as matrix resin, the resin not only retains the excellent effect of capsaicin as an antifouling agent and reduces the use amount of cuprous oxide, but also greatly reduces the irritation of capsaicin in the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of marine coatings, and in particular to a self-polishing antifouling paint and a preparation method thereof. Background Art

[0002] The marine environment is a very complex corrosive and fouling environment. Equipment immersed in seawater is inevitably affected by marine fouling organisms. Marine fouling organisms attach to the surface below the waterline of the ship, which not only affects the performance of the ship, but also causes huge economic losses and waste of resources. Applying antifouling paint is currently the most important way to solve the impact of fouling organisms.

[0003] With the increase of environmental awareness, environmentally friendly antifouling agents have become the focus of research. Capsaicin, as a natural product, has been used as an antifouling agent. At present, most capsaicin antifouling paints are directly added to the paint. For example, a capsaicin antifouling paint disclosed in CN110484139A directly mixes capsaicin with other raw materials to prepare the antifouling paint. However, relevant experiments show that when capsaicin is directly added to produce antifouling paint, the volatilization of capsaicin during the production and construction process will produce strong irritation to the staff, which is not conducive to production and construction. Summary of the invention

[0004] In view of the above problems, the first object of the present invention is to provide a self-polishing antifouling paint, which uses capsaicin-modified acrylic resin as a base resin. The resin not only retains the excellent effect of capsaicin as an antifouling agent and reduces the use of cuprous oxide, but also greatly reduces the irritation of capsaicin during the production process.

[0005] The second object of the present invention is to provide a method for preparing the above-mentioned self-polishing antifouling paint. The antifouling paint prepared by this method has excellent antifouling ability and good physical properties, and can meet the antifouling requirements of various types of marine engineering equipment.

[0006] The first technical solution adopted by the present invention is: a self-polishing antifouling paint, comprising the following components by weight:

[0007] 100 parts of capsaicin modified acrylic resin;

[0008] 40-50 parts of rosin;

[0009] Chlorinated paraffin 10-25 parts;

[0010] 25-30 parts of xylene;

[0011] Cuprous oxide 110-150 parts;

[0012] 35-50 parts of zinc oxide;

[0013] 17-35 parts of copper pyrithione;

[0014] 10-20 parts of talcum powder;

[0015] 15-30 parts of red iron oxide;

[0016] Dispersant 10-15 parts;

[0017] Wherein, the capsaicin modified acrylic resin is prepared by the following method:

[0018] S1: adding xylene to a reaction container; uniformly mixing the monomer mixture and the initiator to obtain a monomer and initiator mixture; dropwise adding the monomer and initiator mixture into the xylene to obtain an acrylic acid prepolymer; the monomer mixture consists of acrylic acid and acrylate monomers;

[0019] S2: adding capsaicin to the acrylic prepolymer, grafting capsaicin to the acrylic prepolymer through an esterification reaction, and obtaining capsaicin-modified acrylic resin.

[0020] Preferably, in step S1, the mass ratio of xylene to the monomer mixture is 1:1.

[0021] Preferably, in step S1, the acrylic acid accounts for 10% to 30% of the total mass of the monomer mixture.

[0022] Preferably, the acrylic acid ester monomer in step S1 is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate and ethyl methacrylate.

[0023] Preferably, the initiator in step S1 is azobisisobutyl cyanide, and the amount of the initiator used is 4% to 10% of the total mass of the monomer mixture.

[0024] Preferably, the step S1 comprises:

[0025] Add xylene into a reaction container, stir and heat to 75° C. to 95° C.; mix the monomer mixture and the initiator evenly to obtain a mixture of monomers and initiators; dropwise add the mixture of monomers and initiators into xylene, continue the reaction for 1 h to 4 h after the dropwise addition for 1 h to 2 h, and obtain an acrylic prepolymer.

[0026] Preferably, the mass ratio of capsaicin to acrylic acid in step S2 is 1:(1-5).

[0027] Preferably, step S2 comprises:

[0028] Capsaicin is added into a reaction container, capsaicin is grafted onto the acrylic prepolymer through an esterification reaction, and the reaction is continued until the solution becomes transparent, and then the temperature is raised to 140° C. to remove water; the reaction is stopped when no water is evaporated out of the reaction container, and capsaicin-modified acrylic resin is obtained.

[0029] The second technical solution adopted by the present invention is: a method for preparing the self-polishing antifouling paint as described in the first technical solution, comprising the following steps:

[0030] S10: weigh each component and set aside;

[0031] S20: capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and a dispersant are mixed, dispersed and filtered to prepare a self-polishing antifouling paint.

[0032] Beneficial effects of the above technical solution:

[0033] (1) The self-polishing antifouling paint disclosed in the present invention adopts capsaicin-modified acrylic resin as a base resin. The resin not only retains the excellent effect of capsaicin as an antifouling agent and reduces the use of cuprous oxide, but also greatly reduces the irritation of capsaicin during the production process.

[0034] (2) The self-polishing antifouling paint provided by the present invention has excellent antifouling ability and good physical properties, and can meet the antifouling requirements of various types of marine engineering equipment.

[0035] (3) Currently commonly used zinc acrylate self-polishing resin and silicon acrylate self-polishing resin only have self-polishing properties, but not anti-fouling properties; although copper acrylate self-polishing resin releases copper ions after hydrolysis, the copper ion content is low and it also does not have anti-fouling properties; the capsaicin modified acrylic resin used in the present invention not only has self-polishing properties, but also has strong anti-fouling properties after the capsaicin on the side chain is hydrolyzed into seawater. Using capsaicin modified acrylic resin as the base resin can effectively reduce the amount of cuprous oxide used.

[0036] (4) Compared with the existing method for preparing capsaicin-modified acrylic resin, the present invention not only retains the antifouling performance of capsaicin by grafting capsaicin onto acrylic resin, but also can significantly reduce the irritation during the antifouling paint coating process, thereby having better antifouling performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The present invention is a process flow chart of a method for preparing a self-polishing antifouling paint. DETAILED DESCRIPTION

[0038] The present invention is further described below through specific embodiments. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the principle of the present invention, and these should also be regarded as belonging to the protection scope of the present invention.

[0039] The contents not described in detail in the specification of the present invention belong to the common knowledge of the professionals in this field.

[0040] The invention discloses a self-polishing antifouling paint, which comprises the following components in parts by weight:

[0041] 100 parts of capsaicin modified acrylic resin;

[0042] 40-50 parts of rosin;

[0043] Chlorinated paraffin 10-25 parts;

[0044] 25-30 parts of xylene;

[0045] Cuprous oxide 110-150 parts;

[0046] 35-50 parts of zinc oxide;

[0047] 17-35 parts of copper pyrithione;

[0048] 10-20 parts of talcum powder;

[0049] 15-30 parts of red iron oxide;

[0050] Dispersant 10-15 parts.

[0051] Wherein, capsaicin modified acrylic resin is prepared by the following method:

[0052] S1: adding xylene to a reaction container, stirring and heating to 75° C. to 95° C.; uniformly mixing the monomer mixture and the initiator to obtain a mixture of monomers and the initiator; dropwise adding the mixture of monomers and the initiator to the xylene, and continuing the reaction for 1 h to 4 h after the dropwise addition for 1 h to 2 h to obtain an acrylic prepolymer;

[0053] The mass ratio of xylene to monomer mixture is 1:1; the monomer mixture is composed of acrylic acid and acrylate monomers, the acrylic acid accounts for 10% to 30% of the total mass of the monomer mixture, and the acrylate monomer is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, and ethyl methacrylate; the initiator is azobisisobutyl cyanide, and the amount of the initiator is 4% to 10% of the total mass of the monomer mixture;

[0054] S2: adding capsaicin into a reaction container, grafting capsaicin with the acrylic acid prepolymer through an esterification reaction, reacting until the solution is transparent and then heating to 140° C. to remove water; stopping the reaction after no water is evaporated from the reaction container to obtain capsaicin-modified acrylic resin; the mass ratio of capsaicin to acrylic acid is 1:(1-5).

[0055] like Figure 1 As shown, the self-polishing antifouling paint is prepared by the following steps:

[0056] S10: Accurately weigh each component in a dry environment and set aside;

[0057] S20: Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, dispersed well and filtered to obtain a self-polishing antifouling paint.

[0058] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test in sea areas according to GB / T 5370.

[0059] Example 1

[0060] A self-polishing antifouling paint comprising the following components in parts by weight:

[0061] 100 parts of capsaicin modified acrylic resin;

[0062] Rosin 50 parts;

[0063] Chlorinated paraffin 10 parts;

[0064] 30 parts of xylene;

[0065] Cuprous oxide 130 parts;

[0066] 40 parts of zinc oxide;

[0067] Copper pyrithione 20 parts;

[0068] 15 parts of talcum powder;

[0069] 20 parts of red iron oxide;

[0070] Dispersant 10 parts.

[0071] Capsaicin modified acrylic resin is prepared according to the following process:

[0072] Step 1: Add 250g of xylene into a reaction container, stir and heat to 75°C; mix 25g of acrylic acid, 75g of methyl methacrylate, 150g of ethyl acrylate monomer mixture and 10g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 2h. After the dropwise addition is completed, continue to react for 4h to obtain an acrylic acid prepolymer;

[0073] Step 2: Add 25g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0074] Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain the self-polishing antifouling paint.

[0075] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test. After 24 months, no obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0076] Example 2

[0077] A self-polishing antifouling paint comprising the following components in parts by weight:

[0078] 100 parts of capsaicin modified acrylic resin;

[0079] 40 parts of rosin;

[0080] Chlorinated paraffin 25 parts;

[0081] 25 parts of xylene;

[0082] Cuprous oxide 110 parts;

[0083] Zinc oxide 50 parts;

[0084] Copper pyrithione 35 parts;

[0085] 20 parts of talcum powder;

[0086] 30 parts of red iron oxide;

[0087] Dispersant 15 parts.

[0088] Capsaicin modified acrylic resin is prepared according to the following process:

[0089] Step 1: Add 250g of xylene into a reaction container, stir and heat to 85°C; mix 75g of acrylic acid, 75g of methyl acrylate, 100g of ethyl methacrylate monomer mixture and 20g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 2h. After the dropwise addition is completed, continue to react for 1h to obtain an acrylic acid prepolymer;

[0090] Step 2: Add 50g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0091] Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain the self-polishing antifouling paint.

[0092] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test. After 24 months, no obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0093] Example 3

[0094] A self-polishing antifouling paint comprising the following components in parts by weight:

[0095] 100 parts of capsaicin modified acrylic resin;

[0096] 45 parts of rosin;

[0097] Chlorinated paraffin 20 parts;

[0098] 25 parts of xylene;

[0099] Cuprous oxide 130 parts;

[0100] 40 parts of zinc oxide;

[0101] Copper pyrithione 20 parts;

[0102] 15 parts of talcum powder;

[0103] 20 parts of red iron oxide;

[0104] Dispersant 13 parts.

[0105] Capsaicin modified acrylic resin is prepared according to the following process:

[0106] Step 1: Add 250g of xylene into a reaction container, stir and heat to 95°C; mix 50g of acrylic acid, 50g of methyl methacrylate, 150g of ethyl acrylate monomer mixture and 15g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 1h. After the dropwise addition is completed, continue to react for 2h to obtain an acrylic acid prepolymer;

[0107] Step 2: Add 20g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0108] Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain the self-polishing antifouling paint.

[0109] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test. After 24 months, no obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0110] Example 4

[0111] A self-polishing antifouling paint comprising the following components in parts by weight:

[0112] 100 parts of capsaicin modified acrylic resin;

[0113] Rosin 50 parts;

[0114] Chlorinated paraffin 10 parts;

[0115] 30 parts of xylene;

[0116] Cuprous oxide 150 parts;

[0117] 35 parts of zinc oxide;

[0118] Copper pyrithione 17 parts;

[0119] 10 parts of talcum powder;

[0120] 15 parts of red iron oxide;

[0121] Dispersant 12 parts.

[0122] Capsaicin modified acrylic resin is prepared according to the following process:

[0123] Step 1: Add 250g of xylene into a reaction container, stir and heat to 80°C; mix 50g of acrylic acid, 175g of methyl acrylate, 25g of ethyl methacrylate monomer mixture and 25g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 1h. After the dropwise addition is completed, continue to react for 1h to obtain an acrylic acid prepolymer;

[0124] Step 2: Add 10g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0125] Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain the self-polishing antifouling paint.

[0126] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test. After 24 months, no obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0127] Example 5

[0128] A self-polishing antifouling paint comprising the following components in parts by weight:

[0129] 100 parts of capsaicin modified acrylic resin;

[0130] Rosin 50 parts;

[0131] Chlorinated paraffin 10 parts;

[0132] 30 parts of xylene;

[0133] Cuprous oxide 120 parts;

[0134] 45 parts of zinc oxide;

[0135] Copper pyrithione 20 parts;

[0136] 13 parts of talcum powder;

[0137] Red iron oxide 17 parts;

[0138] Dispersant 13 parts.

[0139] Capsaicin modified acrylic resin is prepared according to the following process:

[0140] Step 1: Add 250g of xylene into a reaction container, stir and heat to 75°C; mix 75g of acrylic acid, 100g of methyl methacrylate, 75g of ethyl acrylate monomer mixture and 25g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 1h. After the dropwise addition is completed, continue to react for 1h to obtain an acrylic acid prepolymer;

[0141] Step 2: Add 25g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0142] Capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain the self-polishing antifouling paint.

[0143] The prepared self-polishing antifouling paint was subjected to a shallow sea immersion test. After 24 months, no obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0144] Comparative Example 1

[0145] Capsaicin modified acrylic resin is prepared according to the following process:

[0146] Step 1: Add 250g of xylene into a reaction container, stir and heat to 75°C; mix 25g of acrylic acid, 75g of methyl methacrylate, 150g of ethyl acrylate monomer mixture and 5g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 2h. After the dropwise addition is completed, continue to react for 4h to obtain an acrylic acid prepolymer;

[0147] Step 2: Add 25g of capsaicin into a reaction container, graft capsaicin with acrylic prepolymer through esterification reaction, react until the solution is transparent, then heat to 140°C to remove water; stop the reaction when no water is evaporated in the reaction container to obtain capsaicin-modified acrylic resin.

[0148] The capsaicin-modified acrylic resin is in a gel state, has no fluidity, and cannot be used.

[0149] Comparative Example 2

[0150] Capsaicin modified acrylic resin is prepared according to the following process:

[0151] Step 1: Add 250g of xylene into a reaction container, stir and heat to 75°C; mix 25g of acrylic acid, 75g of methyl methacrylate, 150g of ethyl acrylate monomer mixture and 10g of initiator azobisisobutyl cyanide evenly, and then dropwise add to xylene for 2h. After the dropwise addition is completed, continue to react for 4h to obtain an acrylic acid prepolymer;

[0152] Step 2: Add 50 g of capsaicin into a reaction container, and graft capsaicin with acrylic acid prepolymer through esterification reaction. Capsaicin and acrylic acid prepolymer cannot react completely, and finally a white gel mixture is obtained.

[0153] Comparative Example 3

[0154] A self-polishing antifouling paint comprising the following components in parts by weight:

[0155] 100 parts of capsaicin modified acrylic resin;

[0156] Rosin 50 parts;

[0157] Chlorinated paraffin 10 parts;

[0158] 30 parts of xylene;

[0159] Cuprous oxide 130 parts;

[0160] 40 parts of zinc oxide;

[0161] Copper pyrithione 20 parts;

[0162] 15 parts of talcum powder;

[0163] 20 parts of red iron oxide;

[0164] Dispersant 10 parts.

[0165] The capsaicin modified acrylic resin is prepared according to the process disclosed in CN108341909A; the capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and dispersant are fully mixed, well dispersed and filtered to obtain a self-polishing antifouling paint.

[0166] The self-polishing antifouling paint prepared in Comparative Example 3 was subjected to a shallow sea immersion test. After 24 months, obvious marine organisms were attached to the effective area of ​​the test plate surface.

[0167] By comparing the shallow sea hanging boards in Examples 1 to 5 and Comparative Example 3, there is no obvious marine organism attachment within the effective area of ​​the test board surface in Examples 1 to 5, and the result is better; while in Comparative Example 3, there is obvious marine organism attachment on the test board surface; this indicates that the capsaicin-modified acrylic resin prepared by the method disclosed in the present invention has a better anti-fouling effect.

[0168] The present invention has been described in detail, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments; the above description cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, the technical solution of the present invention and its implementation methods can be subjected to a variety of equivalent substitutions, modifications or improvements, all of which fall within the scope of the present invention; the protection scope of the present invention shall be subject to the attached claims.

Claims

1. A self-polishing antifouling paint, characterized in that: The composition includes the following components by weight: 100 parts of capsaicin modified acrylic resin; 40-50 parts of rosin; Chlorinated paraffin 10-25 parts; 25-30 parts of xylene; Cuprous oxide 110-150 parts; 35-50 parts of zinc oxide; 17-35 parts of copper pyrithione; 10-20 parts of talcum powder; 15-30 parts of red iron oxide; Dispersant 10-15 parts; Wherein, the capsaicin modified acrylic resin is prepared by the following method: S1: adding xylene to a reaction container; uniformly mixing the monomer mixture and the initiator to obtain a monomer and initiator mixture; dropwise adding the monomer and initiator mixture into the xylene to obtain an acrylic acid prepolymer; the monomer mixture consists of acrylic acid and acrylate monomers; S2: adding capsaicin to the acrylic prepolymer, grafting capsaicin to the acrylic prepolymer through an esterification reaction, and obtaining capsaicin-modified acrylic resin.

2. The self-polishing antifouling paint according to claim 1, characterized in that The mass ratio of xylene to the monomer mixture in step S1 is 1:

1.

3. The self-polishing antifouling paint according to claim 1, characterized in that In step S1, the acrylic acid accounts for 10% to 30% of the total mass of the monomer mixture.

4. The self-polishing antifouling paint according to claim 1, characterized in that The acrylic acid ester monomer in step S1 is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate and ethyl methacrylate.

5. The self-polishing antifouling paint according to claim 1, characterized in that: The initiator in step S1 is azobisisobutyl cyanide, and the amount of the initiator used is 4% to 10% of the total mass of the monomer mixture.

6. The self-polishing antifouling paint according to claim 1, characterized in that The step S1 comprises: Add xylene into a reaction container, stir and heat to 75° C. to 95° C.; mix the monomer mixture and the initiator evenly to obtain a mixture of monomers and initiators; dropwise add the mixture of monomers and initiators into xylene, continue the reaction for 1 h to 4 h after the dropwise addition for 1 h to 2 h, and obtain an acrylic prepolymer.

7. The self-polishing antifouling paint according to claim 1, characterized in that The mass ratio of capsaicin to acrylic acid in step S2 is 1:(1-5).

8. The self-polishing antifouling paint according to claim 1, characterized in that The step S2 comprises: Capsaicin is added into a reaction container, capsaicin is grafted onto the acrylic prepolymer through an esterification reaction, and the reaction is continued until the solution becomes transparent, and then the temperature is raised to 140° C. to remove water; the reaction is stopped when no water is evaporated out of the reaction container, and capsaicin-modified acrylic resin is obtained.

9. A method for preparing a self-polishing antifouling paint according to any one of claims 1 to 8, characterized in that: The following steps are involved: S10: weigh each component and set aside; S20: capsaicin modified acrylic resin, rosin, chlorinated paraffin, xylene, cuprous oxide, zinc oxide, copper pyrithione, talcum powder, red iron oxide and a dispersant are mixed, dispersed and filtered to prepare a self-polishing antifouling paint.

Citation Information

Patent Citations

  • A marine biofouling paint, its preparation method and application

    CN102300944A

  • Long-acting self-polishing antifouling paint and preparation method thereof

    CN102732122A

  • Antibacterial capsaicin modified acrylic resin as well as preparation method and application thereof

    CN108341909A

  • Acrylic resin containing capsaicin and preparation method thereof

    CN116496440A

Cited By

  • Dual-degradable resin and preparation method thereof, antifouling agent system, marine antifouling composition and application thereof

    CN121851270A