High-temperature-resistant powder coating and preparation method thereof
By combining phenolic epoxy resin with terminal amino adducts, melamine, and high-temperature resistant fillers, the problem of cracking and peeling of powder coatings at high temperatures has been solved, achieving stable use at temperatures above 300℃, making it suitable for high-temperature equipment such as fireplaces and heaters.
Patent Information
- Application Number
- CN202410975836.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing powder coatings are prone to cracking and peeling under high temperature conditions, and cannot meet the high temperature resistance requirements of high-temperature application scenarios such as fireplaces, heaters, and barbecue grills.
Phenolic epoxy resin is used as the base resin, combined with terminal amino adducts, melamine and high-temperature resistant fillers. The terminal amino adducts react with the epoxy resin to form a curing agent. Combined with aminosiloxane and reactive silane coupling agent, the heat resistance and flexibility of the coating are improved, forming a stable coating above 300℃.
The prepared high-temperature resistant powder coating is not damaged when used at temperatures above 300℃, exhibits excellent high-temperature resistance, avoids cracking and peeling, and is suitable for high-temperature applications.
Smart Images

Figure BDA0004954484640000161 
Figure BDA0004954484640000171
Abstract
Description
Technical Field
[0001] The invention relates to the field of powder coatings, and in particular to a high temperature resistant powder coating and a preparation method thereof. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating that usually does not contain solvents. When used, it is sprayed on the surface of the substrate using air as the medium, and then a coating is formed on the surface of the substrate through curing methods such as heating. Therefore, compared with solvent-dispersed coatings, powder coatings have the advantages of being non-toxic and environmentally friendly.
[0003] With the development of powder coatings, powder coatings have also been used in fireplaces, heaters, barbecue grills, frying pans, exhaust pipes, chimneys and other fields in recent years. These fields often involve high-temperature application scenarios, requiring powder coatings to have better high-temperature resistance. The existing ordinary powder coatings cannot meet the high-temperature resistance requirements and are prone to cracking and peeling when used under high temperature conditions. Summary of the invention
[0004] In view of the deficiencies in the prior art, the first object of the present invention is to provide a high temperature resistant powder coating, which has good high temperature resistance and can be used above 300°C without damage.
[0005] The second object of the present invention is to provide a method for preparing the high temperature resistant powder coating, which has the advantages of simple steps and improved coating performance.
[0006] To achieve the first purpose of the present invention, the present invention provides a high temperature resistant powder coating, which includes the following raw materials in parts by mass: 100 parts of phenolic epoxy resin; 20 to 30 parts of terminal amino adduct; 15 to 25 parts of melamine; 80 to 90 parts of high temperature resistant filler; 2 to 5 parts of aminosiloxane; wherein the terminal amino adduct is the reaction product of terminal amino linear polysiloxane and an epoxy mixture, and the epoxy mixture is a mixture of bisphenol A epoxy resin and alicyclic epoxy resin.
[0007] In some embodiments of the present invention, the amino-terminated linear polysiloxane has a number average molecular weight of 1000-1500.
[0008] In some embodiments of the present invention, the bisphenol A epoxy resin is selected from at least one of E44 and E51.
[0009] In some embodiments of the present invention, the alicyclic epoxy resin is selected from at least one of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, and dicyclopentadiene diepoxide.
[0010] In some embodiments of the present invention, the mass ratio of the epoxy mixture to the amino-terminated linear polysiloxane is 1:(3-5).
[0011] In some embodiments of the present invention, the mass ratio of the bisphenol A epoxy resin to the alicyclic epoxy resin is 1:(2-3).
[0012] In some embodiments of the present invention, the phenolic epoxy resin is at least one selected from Epalloy 8240 and Epalloy 8250 produced by CVC.
[0013] In some embodiments of the present invention, the high temperature resistant filler is selected from at least one of ceramics, graphite, alumina, and silica.
[0014] In some embodiments of the present invention, the high temperature resistant powder coating further comprises an additive, and the mass fraction of the additive is 1 to 10 mass fractions relative to 100 mass fractions of the phenolic epoxy resin.
[0015] In some embodiments of the present invention, the additive is selected from at least one of a pigment, a wetting agent, a dispersant, and a curing accelerator.
[0016] To achieve the second purpose of the present invention, the present invention provides a method for preparing a high temperature resistant powder coating as described in any of the above schemes, which comprises the following steps: step one: reacting the epoxy mixture with the amino-terminated linear polysiloxane to obtain an amino-terminated adduct; step two: uniformly mixing the amino-terminated adduct, melamine, a high temperature resistant filler and an aminosiloxane to obtain a curing agent composition; step three: melt-mixing the curing agent composition and a phenolic epoxy resin to obtain a powder.
[0017] In some embodiments of the present invention, in step 2, the terminal amino adduct, aminosiloxane and solvent are mixed to obtain a dispersion, the dispersion is stirred and mixed with melamine and a high temperature resistant filler to be uniformly mixed, and then dried to obtain a curing agent composition; the solvent is a mixture of water and ethanol.
[0018] In some embodiments of the present invention, in the step three, the temperature of the melt mixing is 100-130°C.
[0019] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0020] The high temperature resistant powder coating of the present invention uses phenolic epoxy resin as a base resin, and is combined with terminal amino adduct and melamine as a curing agent, wherein the phenolic epoxy resin contains a phenolic resin segment structure and has good heat resistance; melamine has a triazine ring structure, which can also improve the high temperature resistance; the terminal amino adduct is an adduct of terminal amino linear polysiloxane and bisphenol A epoxy resin and alicyclic epoxy resin, the linear siloxane segment can withstand high temperature and improve the flexibility of the coating, avoid cracking of the coating under high temperature environment, bisphenol A epoxy resin and alicyclic epoxy resin themselves also have good heat resistance, and the mixture of the two can react more fully with terminal amino linear polysiloxane, improve the fluidity of the coating of the terminal amino adduct and the uniformity of the coating obtained, and improve the high temperature resistance of the coating. The present invention also improves the dispersion degree of the filler and the high temperature bearing capacity of the coating by adding high temperature resistant fillers and reactive silane coupling agents. The coating prepared by the high temperature resistant powder coating of the present invention can be used above 300°C without damage, and has good high temperature stability. DETAILED DESCRIPTION
[0021] The embodiment of the present invention provides a high temperature resistant powder coating, which can be used at a high temperature higher than 300°C without blistering, cracking or peeling. The powder coating is suitable for high temperature application scenarios, such as fireplaces, heating stoves, barbecue stoves, frying pan stoves, exhaust pipes, chimneys and other fields.
[0022] Specifically, the high temperature resistant powder coating includes the following raw materials in parts by mass: 100 parts of phenolic epoxy resin; 20 to 30 parts of terminal amino adduct; 15 to 25 parts of melamine; 80 to 90 parts of high temperature resistant filler; 2 to 5 parts of aminosiloxane; wherein the terminal amino adduct is the reaction product of terminal amino linear polysiloxane and epoxy mixture, and the epoxy mixture is a mixture of bisphenol A type epoxy resin and alicyclic epoxy resin. Among them, the phenolic epoxy resin has a phenolic resin structure and carries epoxy groups on the molecular chain, which itself has high heat resistance, and can be further reacted and cured to form a three-dimensional cross-linked network, thereby improving the high temperature resistance of the coating. The terminal amino adduct is obtained by prepolymerization of terminal amino linear polysiloxane, bisphenol A type epoxy resin and alicyclic epoxy resin, and has amino groups at both ends of its molecular chain. The amino group can participate in the curing reaction of the epoxy resin, so the terminal amino adduct can be used as a curing agent; the linear polysiloxane has S iOS i segment, has high heat resistance, good segment flexibility, can rotate flexibly at high temperature, and avoid cracking of coating; bisphenol A epoxy resin structure and alicyclic epoxy resin structure in terminal amino adduct can improve the compatibility of terminal amino adduct and phenolic epoxy resin, and bisphenol A epoxy resin and alicyclic epoxy resin are mixed and used, both of which have good heat resistance, and the mixture of the two can react more fully with terminal amino linear polysiloxane, improve the fluidity of the coating of the terminal amino adduct and the uniformity of the obtained coating, and improve the high temperature resistance of the coating; melamine has primary and tertiary amino groups, can participate in epoxy resin curing well, and has triazine rings on its molecular chain, and has good high temperature resistance; high temperature resistant filler can further improve the heat resistance of the coating, and aminosiloxane can improve the dispersibility of high temperature resistant filler in resin. The present invention obtains a powder coating that can form a coating that can be used for a long time at 300°C through the mutual cooperation of multiple components.
[0023] In some examples, relative to 100 parts by mass of phenolic epoxy resin, the mass of terminal amino adduct can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.; the mass of melamine is 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.; the mass of high temperature resistant filler is 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, etc.; the mass of aminosiloxane is 2 parts, 3 parts, 4 parts, 5 parts, etc. Without departing from the spirit and principle of the present invention, the mass of each raw material can be selected within the above values or within the range therebetween.
[0024] In some examples, the high temperature resistant powder coating is mainly composed of the following raw materials in parts by mass: 100 parts of phenolic epoxy resin; 20-30 parts of terminal amino adduct; 15-25 parts of melamine; 80-90 parts of high temperature resistant filler; 2-5 parts of aminosiloxane. In addition to the phenolic epoxy resin, terminal amino adduct, melamine, high temperature resistant filler and aminosiloxane, the powder coating may also contain other components, and the amount of the other components does not exceed 10% of the total mass of the phenolic epoxy resin, terminal amino adduct, melamine, high temperature resistant filler and aminosiloxane.
[0025] In some examples, the high temperature resistant powder coating is composed of the following raw materials in parts by mass: 100 parts of phenolic epoxy resin; 20 to 30 parts of terminal amino adduct; 15 to 25 parts of melamine; 80 to 90 parts of high temperature resistant filler; 2 to 5 parts of aminosiloxane. In addition to the phenolic epoxy resin, terminal amino adduct, melamine, high temperature resistant filler and aminosiloxane, the powder coating may not contain other components. The raw material composition of the powder coating is simpler and can achieve the desired high temperature resistance effect.
[0026] In some examples, the number average molecular weight of the amino-terminated linear polysiloxane is 1000 to 1500, thereby providing a longer siloxane chain and giving the coating higher heat resistance and flexibility. The amino-terminated linear polysiloxane can be an aminopropyl-dicapped polydimethylsiloxane, that is, aminopropyl groups are connected to both ends of the polydimethylsiloxane molecular chain. The preparation process of the amino-terminated linear polysiloxane is mature and can be purchased commercially.
[0027] In some examples, the bisphenol A epoxy resin is selected from at least one of E44 and E51. The bisphenol A epoxy resin has a higher epoxy value and reacts faster and more fully with the amino-terminated linear polysiloxane.
[0028] In some examples, the alicyclic epoxy resin is selected from at least one of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, and dicyclopentadiene diepoxide. The alicyclic epoxy resin molecules have a six-membered ring and have high heat resistance and chemical stability.
[0029] In some examples, the mass ratio of the epoxy mixture to the amino-terminated linear polysiloxane is 1:(3-5), for example, 1:3, 1:4, 1:5, etc. When the mass ratio of the epoxy mixture to the amino-terminated linear polysiloxane is within the above range, the desired amino-terminated adduct can be obtained, and the molecular weight of the adduct is controlled, thereby improving the fluidity of the powder coating during construction.
[0030] In some examples, the mass ratio of bisphenol A epoxy resin to alicyclic epoxy resin is 1:(2-3), for example, 1:2, 1:2.5, 1:3, etc. When the mass ratio of bisphenol A epoxy resin to alicyclic epoxy resin is within the above range, the viscosity and fluidity of the obtained amino-terminated linear polysiloxane are moderate, which helps the amino-terminated linear polysiloxane to disperse and fully react with the novolac epoxy resin to form a uniform coating film.
[0031] In some examples, the phenolic epoxy resin is selected from at least one of Epalloy 8240 and Epalloy 8250 produced by CVC, and the above phenolic epoxy resin is solid or semi-solid at room temperature, which helps to obtain a solid powder coating with high storage stability. In addition, the above phenolic epoxy resin has a high epoxy value, which can improve the crosslinking density and compactness of the coating, thereby improving the high temperature resistance of the coating.
[0032] In some examples, the high temperature resistant filler is selected from at least one of ceramics, graphite, alumina, and silica. The above fillers have good stability at high temperatures and can improve the high temperature resistance of the coating.
[0033] In some examples, the high temperature resistant powder coating further includes an additive, and the mass portion of the additive is 1 to 10 parts relative to 100 parts by mass of the phenolic epoxy resin, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc. The additive can be selected from at least one of a pigment, a wetting agent, a dispersant, and a curing accelerator, which are used for coloring the coating, improving the wetting of the coating on the substrate, promoting the dispersion of raw materials, and promoting the curing reaction. In some examples, the high temperature resistant powder coating is composed of a phenolic epoxy resin, an amino-terminated adduct, melamine, a high temperature resistant filler, an aminosiloxane, and an additive.
[0034] In some examples, the method for preparing the high temperature resistant powder coating may include the following steps:
[0035] Step 1: react the epoxy mixture with amino-terminated linear polysiloxane to obtain an amino-terminated adduct. In step 1, the epoxy mixture and amino-terminated linear polysiloxane can be uniformly mixed in a solvent such as ethyl acetate, and reacted at about 150-200°C for 16-20 hours. After the reaction is completed, the solvent is recovered by rotary evaporation to obtain an amino-terminated epoxy adduct. The amino-terminated epoxy adduct may contain reaction products of epoxy mixtures with different polymerization degrees and amino-terminated linear polysiloxanes. The amino-terminated epoxy adduct may also contain some unreacted amino-terminated linear polysiloxanes, which do not need to be removed.
[0036] Step 2: Evenly mix the terminal amino adduct, melamine, high temperature resistant filler and aminosiloxane to obtain a curing agent composition. Step 2: First, the terminal amino adduct, melamine and other curing agents and aminosiloxane are mixed with the high temperature resistant filler, which is conducive to evenly dispersing the high temperature resistant filler.
[0037] Step 3: Melt and mix the curing agent composition and the phenolic epoxy resin evenly and make them into powder. After the curing agent composition is evenly mixed, the phenolic epoxy resin is added for melt mixing to avoid excessive crosslinking and curing of the epoxy resin and make the raw materials more fully mixed and more dispersed. In step 3, the curing agent composition and the phenolic epoxy resin are allowed to partially prepolymerize to increase the viscosity of the mixture, which helps to obtain a powder coating that is stable in a solid state at room temperature.
[0038] As can be seen from the above, the preparation method of the high temperature resistant powder coating of the present invention is simple, and the raw material components are fully and evenly mixed, thereby improving the performance of the powder coating.
[0039] In some examples, in step 2, the amino-terminated adduct, aminosilicone and solvent are mixed to obtain a dispersion, and the dispersion is stirred and mixed evenly with melamine and a high temperature resistant filler, and then dried to obtain a curing agent composition. The above steps can disperse the amino-terminated adduct and aminosilicone to the surface of the solid melamine and the high temperature resistant filler, so that the curing agent composition is mixed more evenly, and promote the hydrolysis of aminosilicone and bonding to the filler surface. The solvent can be a mixture of water and ethanol, which is non-toxic, environmentally friendly and easy to recycle.
[0040] In some examples, in step three, the temperature of melt mixing is 100-130° C. The above melt temperature range can make the curing agent composition and the phenolic epoxy resin melt mixed evenly, and the epoxy resin and the curing agent will not be over-cured and cross-linked prematurely.
[0041] In some examples, step three may be performed in an extruder, and the step of making a powder may include granulation and pulverization.
[0042] The present invention will be further described in detail by specific examples. In the following examples and comparative examples, substances with the same name are substances with the same source and the same physical properties. The raw materials are all commercially available or obtained according to conventional processes in the prior art.
[0043] Example 1
[0044] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0045] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0046] 20 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane with a number average molecular weight of 1000 and an epoxy mixture consisting of E44 epoxy resin and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:3, and the mass ratio of the E44 epoxy resin to the 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate is 1:2;
[0047] 15 parts of melamine;
[0048] 90 parts of high temperature resistant filler alumina powder;
[0049] 5 parts of aminopropyltriethoxysilane;
[0050] 3 parts of pigment.
[0051] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0052] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0053] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0054] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0055] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0056] Example 2
[0057] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0058] 100 parts of phenolic epoxy resin Epa ll oy 8250;
[0059] 30 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane with a number average molecular weight of 1500 and an epoxy mixture consisting of E51 epoxy resin and cyclohexane-1,2-dicarboxylic acid diglycidyl ester, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:5, and the mass ratio of the E51 epoxy resin to the cyclohexane-1,2-dicarboxylic acid diglycidyl ester is 1:3;
[0060] 25 parts of melamine;
[0061] 80 parts of high temperature resistant filler silica powder;
[0062] 3 parts of aminopropyltriethoxysilane;
[0063] 3 parts of pigment.
[0064] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0065] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0066] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0067] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0068] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0069] Example 3
[0070] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0071] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0072] 25 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane having a number average molecular weight of 1300 and an epoxy mixture consisting of E44 epoxy resin and dicyclopentadiene diepoxide, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:4, and the mass ratio of the E44 epoxy resin to the dicyclopentadiene diepoxide is 1:2.5;
[0073] 20 parts of melamine;
[0074] 85 parts of high temperature resistant filler ceramic powder;
[0075] 2 parts of aminopropyltriethoxysilane;
[0076] 3 parts of pigment.
[0077] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0078] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0079] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0080] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0081] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0082] Example 4
[0083] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0084] 100 parts of phenolic epoxy resin Epa ll oy 8250;
[0085] 30 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane with a number average molecular weight of 1500 and an epoxy mixture consisting of E51 epoxy resin and cyclohexane-1,2-dicarboxylic acid diglycidyl ester, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:7, and the mass ratio of the E51 epoxy resin to the cyclohexane-1,2-dicarboxylic acid diglycidyl ester is 1:3;
[0086] 25 parts of melamine;
[0087] 80 parts of high temperature resistant filler alumina powder;
[0088] 3 parts of aminopropyltriethoxysilane;
[0089] 3 parts of pigment.
[0090] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0091] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0092] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0093] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0094] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0095] Example 5
[0096] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0097] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0098] 25 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane having a number average molecular weight of 1300 and an epoxy mixture consisting of E44 epoxy resin and dicyclopentadiene diepoxide, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:4, and the mass ratio of the E44 epoxy resin to the dicyclopentadiene diepoxide is 1:6;
[0099] 20 parts of melamine;
[0100] 85 parts of high temperature resistant filler ceramic powder;
[0101] 2 parts of aminopropyltriethoxysilane;
[0102] 3 parts of pigment.
[0103] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0104] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0105] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0106] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0107] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0108] Comparative Example 1
[0109] The raw materials of the powder coating of this comparative example are as follows:
[0110] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0111] 40 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane with a number average molecular weight of 1000 and an epoxy mixture consisting of E44 epoxy resin and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, wherein the mass ratio of the epoxy mixture to the aminopropyl di-terminated polydimethylsiloxane is 1:3, and the mass ratio of the E44 epoxy resin to the 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate is 1:2;
[0112] 5 parts of melamine;
[0113] 90 parts of high temperature resistant filler alumina powder;
[0114] 5 parts of aminopropyltriethoxysilane;
[0115] 3 parts of pigment.
[0116] The preparation method of the powder coating of this comparative example has the following steps:
[0117] Step 1: Evenly mix the epoxy mixture and aminopropyl dicapped polydimethylsiloxane in ethyl acetate, react at 180° C. for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0118] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0119] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0120] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0121] Comparative Example 2
[0122] The raw materials of the powder coating of this comparative example are as follows:
[0123] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0124] 20 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl-dicapped polydimethylsiloxane having a number average molecular weight of 1000 and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, wherein the mass ratio of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate to the aminopropyl-dicapped polydimethylsiloxane is 1:3;
[0125] 15 parts of melamine;
[0126] 90 parts of high temperature resistant filler alumina powder;
[0127] 5 parts of aminopropyltriethoxysilane;
[0128] 3 parts of pigment.
[0129] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0130] Step 1: 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate and aminopropyl dicapped polydimethylsiloxane are mixed evenly in ethyl acetate, reacted at 180° C. for 18 hours, and after the reaction is completed, the solvent is removed by rotary evaporation to obtain an amino-terminated adduct;
[0131] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0132] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0133] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0134] Comparative Example 3
[0135] The raw materials of the powder coating of this comparative example are as follows:
[0136] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0137] 20 parts of an amino-terminated adduct, which is obtained by prepolymerizing an aminopropyl di-terminated polydimethylsiloxane with a number average molecular weight of 1000 and an E44 epoxy resin, wherein the mass ratio of the E44 epoxy resin to the aminopropyl di-terminated polydimethylsiloxane is 1:3;
[0138] 15 parts of melamine;
[0139] 90 parts of high temperature resistant filler alumina powder;
[0140] 5 parts of aminopropyltriethoxysilane;
[0141] 3 parts of pigment.
[0142] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0143] Step 1: E44 epoxy resin and aminopropyl dicapped polydimethylsiloxane are mixed evenly in ethyl acetate, reacted at 180° C. for 18 hours, and after the reaction is completed, the solvent is removed by rotary evaporation to obtain an amino-terminated adduct;
[0144] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0145] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0146] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0147] Comparative Example 4
[0148] The raw materials of the high temperature resistant powder coating of this embodiment are as follows:
[0149] 100 parts of phenolic epoxy resin Epa ll oy 8240;
[0150] 20 parts of an amino-terminated adduct, which is obtained by prepolymerizing p-phenylenediamine with an epoxy mixture consisting of E44 epoxy resin and 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, wherein the mass ratio of the epoxy mixture to p-phenylenediamine is 1:1, and the mass ratio of the E44 epoxy resin to the 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate is 1:2;
[0151] 15 parts of melamine;
[0152] 90 parts of high temperature resistant filler alumina powder;
[0153] 5 parts of aminopropyltriethoxysilane;
[0154] 3 parts of pigment.
[0155] The steps of the preparation method of the high temperature resistant powder coating of this embodiment are as follows:
[0156] Step 1: Evenly mix the epoxy mixture and p-phenylenediamine in ethyl acetate, react at 180°C for 18 hours, and remove the solvent by rotary evaporation after the reaction to obtain an amino-terminated adduct;
[0157] Step 2: Evenly mix the amino-terminated adduct, aminopropyltriethoxysilane and a mixture of water and ethanol (volume ratio 1:1) to obtain a dispersion, and evenly mix the dispersion with melamine, a high temperature resistant filler and a pigment, and then vacuum heat and dry to obtain a curing agent composition;
[0158] Step 3: melt and mix the curing agent composition and the phenolic epoxy resin in an extruder at 130° C. to obtain a powder coating.
[0159] The obtained powder coating was sprayed onto the surface of the stainless steel plate and then baked at 160°C for 1 h to obtain a coating thickness of about 0.5 mm.
[0160] Performance Testing
[0161] The terminal amino adducts prepared in the above examples and comparative examples were tested for viscosity at a test temperature of 25°C. The coatings prepared in the above examples and comparative examples were tested for adhesion with reference to GB9286-98; the coatings were tested for thermogravimetric testing at a heating rate of 10°C / min to obtain the temperature corresponding to 10% weight loss of the coating; the coatings were tested for long-term high temperature resistance with reference to GB / T 1735-2009, the test duration was 60 days, and the coatings were treated at 300°C for 10 hours every day to observe the changes in the coatings; after the long-term high temperature resistance test, the undamaged coating parts were taken and the coating adhesion was tested with reference to GB9286-98.
[0162] The test results are shown in Table 1 below.
[0163] Table 1 Test results of embodiments and comparative examples
[0164]
[0165]
[0166] From the test results of the above embodiments and comparative examples, it can be seen that the terminal amino adduct of the present invention has a suitable viscosity, and the obtained high temperature resistant powder coating has good adhesion to the substrate and can withstand high temperatures, and the temperature of 10% thermal decomposition is above 350°C, and can be used above 300°C without damage. The high temperature resistant powder coating of the present invention is suitable for high temperature application scenarios.
[0167] Finally, it should be emphasized that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high temperature resistant powder coating, Features The invention comprises the following raw materials in parts by weight: 100 parts of phenolic epoxy resin; 20-30 parts of terminal amino adduct; 15-25 parts of melamine; 80-90 parts of high temperature resistant filler; 2-5 parts of aminosilicone; The amino-terminated adduct is a reaction product of amino-terminated linear polysiloxane and an epoxy mixture, and the epoxy mixture is a mixture of bisphenol A epoxy resin and alicyclic epoxy resin.
2. A high temperature resistant powder coating according to claim 1, Features: The number average molecular weight of the amino-terminated linear polysiloxane is 1000-1500.
3. A high temperature resistant powder coating according to claim 2, Features: The bisphenol A epoxy resin is selected from at least one of E44 and E51; The alicyclic epoxy resin is selected from at least one of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, and dicyclopentadiene diepoxide.
4. A high temperature resistant powder coating according to claim 3, Features: The mass ratio of the epoxy mixture to the amino-terminated linear polysiloxane is 1:(3-5); The mass ratio of the bisphenol A epoxy resin to the alicyclic epoxy resin is 1:(2-3).
5. A high temperature resistant powder coating according to any one of claims 1 to 4, Features: The phenolic epoxy resin is selected from at least one of Epalloy 8240 and Epalloy 8250 produced by CVC.
6. A high temperature resistant powder coating according to any one of claims 1 to 4, Features: The high temperature resistant filler is selected from at least one of ceramics, graphite, alumina and silicon dioxide.
7. A high temperature resistant powder coating according to any one of claims 1 to 4, Features: The high temperature resistant powder coating further comprises an additive, wherein the mass portion of the additive is 1 to 10 parts relative to 100 parts by mass of the phenolic epoxy resin; The additive is selected from at least one of a pigment, a wetting agent, a dispersant, and a curing accelerator.
8. A method for preparing a high temperature resistant powder coating according to any one of claims 1 to 7, Features The following steps are involved: Step 1: reacting the epoxy mixture with the amino-terminated linear polysiloxane to obtain an amino-terminated adduct; Step 2: Evenly mix the amino-terminated adduct, melamine, high temperature resistant filler and aminosiloxane to obtain a curing agent composition; Step 3: Melt and mix the curing agent composition and the phenolic epoxy resin evenly and prepare into powder.
9. A method for preparing a high temperature resistant powder coating according to claim 8, Features: In the step 2, the amino-terminated adduct, aminosiloxane and solvent are mixed to obtain a dispersion, the dispersion is stirred and mixed with melamine and a high temperature resistant filler to be uniformly mixed, and then dried to obtain a curing agent composition; The solvent is a mixture of water and ethanol.
10. A method for preparing a high temperature resistant powder coating according to claim 8 or 9, Features: In the step three, the temperature of the melt mixing is 100-130°C.
Citation Information
Patent Citations
Dual-cure epoxy-siloxane coating compositions
CN110637068A
Super-hydrophobic powder coating as well as preparation method and coating thereof
CN117625010A
Durable high-temperature-resistant steam enamel powder coating as well as preparation method and application thereof
CN118126604A
Corrosion-resistant epoxy resin powder coating and preparation method thereof
CN118165622A
Copolymers of epoxy compounds and amino silanes
US20140235885A1
Cited By
Open fire resistant powder coating as well as preparation method and application thereof
CN119736003A
Powder coating as well as preparation method and application thereof
CN120310387A