Hot stamping gum and preparation method thereof
By using components such as aqueous acrylic resin, aqueous EVA resin and other components in hot stamping adhesive, combined with specific process treatment, the problem of oxidation corrosion and insufficient adhesion on the surface of paper substrates is solved, and the problem of traditional hot stamping adhesives is insufficient. High adhesion and easy scratching effect improve the clarity and stability of the stamping.
Patent Information
- Application Number
- CN202411163965.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional hot stamping adhesives are prone to oxidation corrosion on the surface of paper substrates, which affects the appearance effect and is difficult to achieve both high adhesion and easy scratching properties of hot stamping pictures and texts.
The combination dispensing formula of aqueous acrylic resin, aqueous EVA resin, aqueous urea formaldehyde resin, water wax emulsion, antioxidant, anti-skin agent, silica powder, PH buffer and diluent is used to form a specific proportion and process. A new hot stamping adhesive is used to enhance the bonding strength and hydrophobicity and inhibit oxidative corrosion.
It effectively solves the problem of easy oxidation and corrosion on the surface of paper products, achieves high adhesion and easy scratching hot stamping performance, and improves the clarity and stability of hot stamping.
Smart Images

Figure BDA0005007286130000031 
Figure BDA0005007286130000041
Abstract
Description
Technical Field
[0001] The invention relates to a hot stamping adhesive and a preparation method thereof, belonging to the technical field of heat transfer. Background Art
[0002] In heat transfer technology, hot stamping adhesive is the main material that effectively bonds with the substrate. However, due to the limitations of existing technology, traditional hot stamping adhesive only focuses on the strength of hot stamping bonding with the substrate, while ignoring the fact that hot stamping images and texts in some special fields need to be scraped after hot stamping. At the same time, due to factors such as the application environment, the material of the substrate, and the traditional hot stamping adhesive technology, the hot stamping foil is prone to occasional oxidation corrosion to varying degrees after being stamped on the surface of some paper substrates, affecting the appearance.
[0003] The present invention adopts water-based acrylic resin, water-based EVA resin, water-based urea-formaldehyde resin, water wax emulsion, antioxidant, anti-skinning agent, silica powder, pH buffer, and diluent as component formulas and innovates, thereby effectively solving the problem of easy oxidation corrosion of hot stamping images and texts on the surface of paper products, and at the same time achieving two application properties of hot stamping with high adhesion on the surface of paper products and hot stamping with images and texts that are easy to scratch. The entire component formula is determined in combination with the characteristics of the technical application and the expected beneficial effects, among which: water-based acrylic resin is the main component that effectively bonds with paper products during the hot stamping process, and its relative proportion in the formula has an important influence on the bonding strength of the hot stamping graphics; water-based EVA, water-based urea-formaldehyde resin, and water-wax emulsion can reduce the bonding strength between the hot stamping adhesive and paper products, and are the key to achieving the easy-to-scratch hot stamping performance of graphics. Among them, water-wax emulsion can also enhance the hydrophobicity of the adhesive, which is effective in preventing oxidation corrosion of the hot stamping graphics; the antioxidant is a mixture of phenolic resin, 2,6-di-tert-butylphenol, and phosphite in a certain proportion, and the action mechanism is complementary, which has a good inhibitory effect on the main inducing factors of oxidation corrosion. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and provide a hot stamping adhesive and its preparation method which can effectively solve the problem that hot stamping images and texts are easily oxidized and corroded on the surface of paper products, has the characteristics of high hot stamping clarity and stable hot stamping, and can achieve two application properties of high adhesion hot stamping on the surface of paper products and easy-to-scratch hot stamping of images and texts.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] A hot stamping adhesive, characterized in that the component formula and its weight parts are: 8-15 parts of water-based acrylic resin, 1-6 parts of water-based EVA, 0-5 parts of water-based urea-formaldehyde resin, 0-5 parts of water-wax emulsion, 2-6 parts of antioxidant, 0-3 parts of anti-skinning agent, 1-5 parts of silicon dioxide powder, 0-2 parts of pH buffer, and 50-90 parts of diluent.
[0007] The molecular weight of the water-based acrylic resin is 1000-2000 and the softening point is 105°C; the water-based EVA is an ultra-low melt index EVA with an MI of 1.5g / 10min and a softening point of 60°C; the molecular weight of the water-based urea-formaldehyde resin is 300-500 and the softening point is 65°C; the water wax emulsion is an anionic paraffin emulsion with a solid content of 60±1% and an average softening point of 60°C; the antioxidant is a mixture of phenolic resin, 2,6-di-tert-butylphenol and phosphite in a mass ratio of 3:3:2, wherein the softening point of the phenolic resin is 65°C and the phosphorus content of the phosphite is 20±1%; the anti-skinning agent is methyl ethyl ethyl ketoxime; the average particle size of the silica powder is 4-6μm and the specific surface area is 40-42m 2 / g; the pH buffer is N-(2-acetamido)-2-aminoethanesulfonic acid; the diluent is a mixture of ethanol, water and isopropanol in a mass ratio of 7:6:1.
[0008] A method for preparing hot stamping adhesive, characterized in that the steps are as follows:
[0009] (1) Prepare materials: prepare materials according to component formula and weight;
[0010] (2) Blending: First, add the silica powder to the diluent in batches under low-speed stirring. After the addition is completed, stir at a speed of 50-80 r / min for 5 minutes, and then continue to stir at a speed of 120-150 r / min for 5 minutes; secondly, add the water wax emulsion in batches under a stirring speed of 50-80 r / min. After the addition is completed, continue to stir at a speed of 100-130 r / min for 3 minutes, and let it stand until the temperature of the mixture stabilizes; then, under a stirring speed of 50-80 r / min, add the water-based acrylic resin, water-based EVA, water-based urea-formaldehyde resin, antioxidant, anti-skinning agent, and pH buffer in batches in turn. After all the additions are completed, continue to stir at a speed of 100-130 r / min for 10 minutes; finally, stop stirring and let it stand for 1-2 hours at a controlled temperature of 20-30°C;
[0011] (3) Filter and reserve: Use a 100-mesh filter to filter and obtain the backing adhesive.
[0012] Compared with the prior art, the present invention can effectively solve the problem that hot stamped images and texts are easily oxidized and corroded on the surface of paper products. It has the characteristics of high hot stamping clarity and stable hot stamping. At the same time, it can achieve two application performances of hot stamping with high adhesion on the surface of paper products and hot stamping with images and texts that are easy to scratch. DETAILED DESCRIPTION
[0013] The present invention is described in detail below in conjunction with specific embodiments:
[0014] Example 1
[0015] The present invention provides a hot stamping adhesive and a preparation method thereof, wherein the component formula and weight parts thereof are:
[0016]
[0017] The molecular weight of the water-based acrylic resin is 1000-2000 and the softening point is 105°C; the water-based EVA is an ultra-low melt index EVA with an MI of 1.5g / 10min and a softening point of 60°C; the antioxidant is a mixture of phenolic resin, 2,6-di-tert-butylphenol and phosphite in a mass ratio of 3:3:2, wherein the softening point of the phenolic resin is 65°C and the phosphorus content of the phosphite is 20±1%; the anti-skinning agent is methyl ethyl ethyl ketoxime; the average particle size of the silicon dioxide powder is 4-6μm and the specific surface area is 40-42m 2 / g; the pH buffer is N-(2-acetamido)-2-aminoethanesulfonic acid; the diluent is a mixture of ethanol, water and isopropanol in a mass ratio of 7:6:1.
[0018] The preparation method steps are:
[0019] (1) Prepare materials: prepare materials according to component formula and weight;
[0020] (2) Blending: First, add the silica powder to the diluent in batches under low-speed stirring. After the addition is completed, stir at a speed of 50-80 r / min for 5 minutes, and then continue to stir at a speed of 120-150 r / min for 5 minutes; secondly, add the water wax emulsion in batches under a stirring speed of 50-80 r / min. After the addition is completed, continue to stir at a speed of 100-130 r / min for 3 minutes, and let it stand until the temperature of the mixture stabilizes; then, under a stirring speed of 50-80 r / min, add the water-based acrylic resin, water-based EVA, water-based urea-formaldehyde resin, antioxidant, anti-skinning agent, and pH buffer in batches in turn. After all the additions are completed, continue to stir at a speed of 100-130 r / min for 10 minutes; finally, stop stirring and let it stand for 1-2 hours at a controlled temperature of 20-30°C;
[0021] (3) Filter and reserve: Use a 100-mesh filter to filter and obtain the backing adhesive.
[0022] Example 2
[0023] The present invention provides a hot stamping adhesive and a preparation method thereof, wherein the component formula and weight parts thereof are:
[0024]
[0025] The molecular weight of the water-based acrylic resin is 1000-2000 and the softening point is 105°C; the water-based EVA is an ultra-low melt index EVA with an MI of 1.5g / 10min and a softening point of 60°C; the molecular weight of the water-based urea-formaldehyde resin is 300-500 and the softening point is 65°C; the water wax emulsion is an anionic paraffin emulsion with a solid content of 60±1% and an average softening point of 60°C; the antioxidant is a mixture of phenolic resin, 2,6-di-tert-butylphenol and phosphite in a mass ratio of 3:3:2, wherein the softening point of the phenolic resin is 65°C and the phosphorus content of the phosphite is 20±1%; the anti-skinning agent is methyl ethyl ethyl ketoxime; the average particle size of the silica powder is 4-6μm and the specific surface area is 40-42m 2 / g; the pH buffer is N-(2-acetamido)-2-aminoethanesulfonic acid; the diluent is a mixture of ethanol, water and isopropanol in a mass ratio of 7:6:1.
[0026] The preparation method steps are:
[0027] (1) Prepare materials: prepare materials according to component formula and weight;
[0028] (2) Blending: First, add the silica powder to the diluent in batches under low-speed stirring. After the addition is completed, stir at a speed of 50-80 r / min for 5 minutes, and then continue to stir at a speed of 120-150 r / min for 5 minutes; secondly, add the water wax emulsion in batches under a stirring speed of 50-80 r / min. After the addition is completed, continue to stir at a speed of 100-130 r / min for 3 minutes, and let it stand until the temperature of the mixture stabilizes; then, under a stirring speed of 50-80 r / min, add the water-based acrylic resin, water-based EVA, water-based urea-formaldehyde resin, antioxidant, anti-skinning agent, and pH buffer in batches in turn. After all the additions are completed, continue to stir at a speed of 100-130 r / min for 10 minutes; finally, stop stirring and let it stand for 1-2 hours at a controlled temperature of 20-30°C;
[0029] (3) Filter and reserve: Use a 100-mesh filter to filter and obtain the backing adhesive.
[0030] The hot stamping adhesive prepared by the above embodiment can be applied to various types of hot stamping foils, can effectively solve the problem that the hot stamping images and texts are easily oxidized and corroded on the surface of paper products, has the characteristics of high hot stamping clarity and stable hot stamping, and can achieve two application performances: high adhesion hot stamping on the surface of paper products and easy-to-scratch hot stamping of images and texts.
[0031] Comprehensive test results are analyzed: (1) In the component formula of Example 1, water-based acrylic resin that can effectively bond with paper products and has excellent bonding strength is used as the main component, and no water-based urea-formaldehyde resin or water wax emulsion is added. A small amount of water-based EVA and an appropriate amount of silica powder can improve the clarity of hot stamping and make the back adhesive layer have a certain smoothness; for this reason, while solving the problem of easy oxidation and corrosion of hot stamping images on the surface of paper products, Example 1 can achieve the performance of high adhesion hot stamping on the surface of paper products; the flat hot stamping temperature is more appropriately controlled at 120-135°C; the round hot stamping temperature is preferably controlled at 170-210°C (specifically adjusted according to the hot stamping speed); (2) Component formula of Example 2 In the method, the addition amount of water-based acrylic resin is controlled at a relatively low percentage, and the addition amount of water-based EVA, water-based urea-formaldehyde resin and water wax emulsion is controlled at a relatively high percentage, which reduces the bonding strength and adhesion between the hot stamping adhesive and the paper product; in addition, a higher addition amount of silica powder is very helpful in reducing the film-forming property of the adhesive while improving the clarity of the hot stamping; for this reason, implementation 2 can solve the problem of easy oxidation and corrosion of the hot stamping graphics on the surface of paper products, while achieving the performance of easy scratch hot stamping of graphics on the surface of paper products; it is more appropriate to control the flat hot stamping temperature at 85-100℃; the round hot stamping temperature should be controlled at 130-160℃ (specific adjustment according to the hot stamping speed).
[0032] The above is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, the present invention may also have several modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the scope of the creative concept of the present invention shall be included in the protection scope of the present invention.
Claims
1. A hot stamping adhesive, characterized in that: The component formula and its weight parts are: 8-15 parts of water-based acrylic resin, 1-6 parts of water-based EVA, 0-5 parts of water-based urea-formaldehyde resin, 0-5 parts of water wax emulsion, 2-6 parts of antioxidant, 0-3 parts of anti-skinning agent, 1-5 parts of silicon dioxide powder, 0-2 parts of pH buffer, and 50-90 parts of diluent.
2. The hot stamping adhesive according to claim 1, characterized in that: The molecular weight of the water-based acrylic resin is 1000-2000 and the softening point is 105°C; the water-based EVA is an ultra-low melt index EVA with an MI of 1.5g / 10min and a softening point of 60°C; the molecular weight of the water-based urea-formaldehyde resin is 300-500 and the softening point is 65°C; the water wax emulsion is an anionic paraffin emulsion with a solid content of 60±1% and an average softening point of 60°C; the antioxidant is a mixture of phenolic resin, 2,6-di-tert-butylphenol and phosphite in a mass ratio of 3:3:2, wherein the softening point of the phenolic resin is 65°C and the phosphorus content of the phosphite is 20±1%; the anti-skinning agent is methyl ethyl ethyl ketoxime; the average particle size of the silica powder is 4-6μm and the specific surface area is 40-42m 2 / g; the pH buffer is N-(2-acetamido)-2-aminoethanesulfonic acid; the diluent is a mixture of ethanol, water and isopropanol in a mass ratio of 7:6:
1.
3. A method for preparing the hot stamping adhesive as claimed in claim 1, characterized in that: The steps are as follows: (1) Prepare materials: prepare materials according to component formula and weight; (2) Blending: First, add the silica powder to the diluent in batches under low-speed stirring. After the addition is completed, stir at a speed of 50-80 r / min for 5 minutes, and then continue to stir at a speed of 120-150 r / min for 5 minutes; secondly, add the water wax emulsion in batches under a stirring speed of 50-80 r / min. After the addition is completed, continue to stir at a speed of 100-130 r / min for 3 minutes, and let it stand until the temperature of the mixture stabilizes; then, under a stirring speed of 50-80 r / min, add the water-based acrylic resin, water-based EVA, water-based urea-formaldehyde resin, antioxidant, anti-skinning agent, and pH buffer in batches in turn. After all the additions are completed, continue to stir at a speed of 100-130 r / min for 10 minutes; finally, stop stirring and let it stand for 1-2 hours at a controlled temperature of 20-30°C; (3) Filter and reserve: Use a 100-mesh filter to filter and obtain the backing adhesive.
Citation Information
Patent Citations
Water-based low-temperature heat transfer printing adhesive and preparation method thereof
CA3130987A1
Holography positioning alumite high speed thermoprint back glue and preparation method
CN101343522A
Thermoprinting adhesive for high-tenacity rubbing-resisting alumite and preparation method of thermoprinting adhesive
CN103849263A
Aqueous anti-slip composition and molded product
JP2002363886A