Casing type biomass charcoal-electricity co-production method and device coupled with CO2 membrane separation
By in-situ gasifying biomass within the anode layer of a tubular SOFC and combining it with CO2 membrane separation, the problem of low coupling efficiency between biomass gasification and SOFC is solved, achieving efficient energy utilization and high-temperature selective application of syngas.
Patent Information
- Application Number
- CN202411018611.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
Existing biomass gasification technologies face problems such as low energy utilization and difficulty in removing tar. The coupling efficiency between biomass gasification and SOFC power generation is not ideal, and energy is not utilized in a cascade manner. The coupling power generation efficiency of SOFC needs to be improved, and it is difficult to achieve selective upgrading and utilization of high-temperature exhaust gas.
The co-firing method of biomass cogeneration using coupled CO2 membrane separation involves pre-filling biomass into the anode layer of a tubular SOFC for gasification, and then upgrading it through a CO2 ceramic membrane. This achieves in-situ gasification of biomass within the anode layer and SOFC power generation, while recycling the high-temperature exhaust gas.
It significantly improves energy utilization and syngas production yield, increases the power density of SOFC, and enables selective application of high-temperature syngas and efficient energy cascade utilization.
Smart Images

Figure CN118909667A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomass energy utilization, and relates to a multi-field and multi-technical implementation method and system construction of biomass gasification, SOFC, and CO2 membrane separation. Background Art
[0002] Renewable energy is an important development direction for the future transformation of traditional energy and exploration of new energy. Biomass energy is the energy form of solar energy stored in biomass in the form of chemical energy. The biomass power generation market is vast. In recent years, the number of biomass power generation installed capacity in the country, including agricultural and forestry biomass power generation and domestic waste incineration power generation, has continued to rise.
[0003] At present, the main methods of biomass energy utilization include biomass power generation, biomass liquid fuel, pyrolysis gasification and other methods; gasification can produce combustible gases containing hydrogen, carbon monoxide, methane, etc. The generated combustible gases can be enriched and used as high-grade fuel to supply gas turbines and other equipment for power generation.
[0004] The gasification process produces tar, which pollutes the environment and gasification equipment, and is an urgent problem to be solved. The fuel gas currently suffers from severe heat loss during utilization.
[0005] Solid oxide fuel cells can efficiently convert chemical energy into electrical energy and are not restricted by the Carnot limit of thermal engines. As an efficient and clean energy conversion technology, they have attracted much attention in the energy field in recent years. However, due to their high-temperature working environment, they often require additional energy supply, have limited application scenarios, and are accompanied by problems such as large heat losses. Summary of the invention
[0006] The existing biomass gasification technology faces the problems of low energy utilization and difficult tar removal. The purpose of the present invention is to propose a shell-and-tube biomass carbon-electricity cogeneration method coupled with CO2 membrane separation, aiming to provide a method with excellent capacity cascade utilization, excellent power generation efficiency and carbon dioxide capture and quality improvement.
[0007] The second object of the present invention is to provide a shell-and-tube biomass charcoal power cogeneration device coupled with CO2 membrane separation for implementing the method.
[0008] There are some biomass gasification and SOFC coupling processes in the prior art, but the coupling efficiency of biomass gasification and SOFC power generation in the existing methods is not ideal, and the energy is not utilized in a cascade manner. The SOFC coupling power generation efficiency needs to be improved. Not only that, it is also difficult to achieve the selective quality improvement of high-temperature tail gas. In view of this problem, the present invention has provided the following improvement plan after research:
[0009] A shell-and-tube biomass carbon power cogeneration method coupled with CO2 membrane separation, wherein biomass is pre-loaded in the anode chamber of the anode layer of a tubular SOFC (i.e., in the inner cavity of the anode layer), and then the tubular SOFC is heated to gasify the biomass in the anode chamber to form synthesis gas and directly contact the anode layer to participate in SOFC power generation; and then the tail gas generated in the power generation stage is upgraded through a CO2 ceramic membrane.
[0010] The present invention provides a new coupling idea of biomass gasification and SOFC power generation, which innovatively gasifies the biomass in situ in the inner cavity of the anode layer of the tubular SOFC and directly reacts with the anode layer for SOFC power generation, which can unexpectedly improve the energy utilization rate, improve the coupling efficiency and effect of the two, significantly improve the preparation yield of synthesis gas, improve the power density of SOFC, and also help to achieve the selective application of high-temperature synthesis gas.
[0011] In the present invention, the tubular SOFC can be a conventional tubular SOFC device. For example, the tubular SOFC includes an anode layer arranged in a hollow tubular shape, an electrolyte layer composited on the surface of the anode layer, and a cathode layer composited on the surface of the electrolyte layer; the inner cavity of the hollow tubular is the anode chamber.
[0012] In the present invention, the inner diameter of the tubular SOFC is 5-30 mm, the thickness of the anode layer is 0.5-2 mm, the thickness of the electrolyte is 0.01-0.1 mm, and the thickness of the cathode layer is 0.01-0.1 mm.
[0013] In the present invention, the material of the anode layer can be known in the industry, for example, it includes Pt, Ag, LaNiO3, La 0.45 Sr 0.45 Ti 0.90 Ni 0.10 O 3-δ , NiO-YSZ, Ni-Ba-CeO3 / BaZrO3, NiO-Gd 0.1 Ce 0.9 O 2-δ At least one of;
[0014] In the present invention, the material of the electrolyte layer can be well known in the industry, for example, it includes 8YSZ, Ce 0.8 Sm 0.2 O 2-δ (SDC), Gd 0.1 Ce 0.9 O 2-δ (GDC), Ce 0.8 G 0.2 O 2-δ (CGO), (Bi 0.75 Y 0.25 )1.86 Ce 0.14 O 3±δ At least one of;
[0015] In the present invention, the material of the cathode layer includes Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O 3-δ ,La 1-x Sr x CoO 3-δ ,La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ 、(La,Sr)MnO 3-δ 、LaSrCoO 4±δ , Mn 1.3 Co 1.3 Cu 0.4 At least one of O4.
[0016] In the present invention, the biomass may be any biological organic matter, for example, at least one of agricultural and forestry waste, wet garbage, and industrial waste;
[0017] In the present invention, a gasifying agent is introduced into the anode chamber to gasify the biomass therein to form synthesis gas;
[0018] In the present invention, the gasifying agent can be any component that can gasify biomass to form synthesis gas, for example, at least one of air, oxygen, nitrogen, and water vapor; further, it can be a mixture of oxygen and water vapor. Further, the flow ratio of water vapor to oxygen can be 0.5 to 2:10. In addition, the oxygen therein is 5 to 50% of the oxygen required for complete combustion of biomass, and considering the cost, it can be further 5 to 15%.
[0019] In the present invention, during the SOFC power generation stage, the synthesis gas formed in the anode chamber directly participates in the anode reaction with the anode layer medium, and the oxygen-containing atmosphere contacts the cathode surface for cathode reaction, thereby achieving SOFC power generation.
[0020] In the present invention, the heating temperature of the tubular SOFC is 650-800° C., and further 730-780° C. Studies have shown that under the efficient coupling of biomass gasification and SOFC, further through the control of the temperature, the coupling efficiency of biomass gasification and SOFC can be further enhanced, and the gasification efficiency and the power of SOFC can be improved.
[0021] In the present invention, the open circuit voltage of the SOFC in the power generation stage is between 0.9V and 1.1V.
[0022] In the present invention, the CO2 ceramic membrane includes a ceramic phase matrix and carbonate compounded therein;
[0023] Preferably, the ceramic phase matrix comprises La 1.5 Sr 0.5 NiO 4+δ ,La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ , Gd 0.2 Ce 0.8 O 2+δ At least one of;
[0024] Preferably, the carbonate includes at least one of Li2CO3, Na2CO3, and K2CO3, and may further be a complex thereof;
[0025] Preferably, the carbonate content in the CO2 ceramic membrane is 30-60%.
[0026] In the present invention, the CO2 ceramic membrane is prepared by the following steps: a gadolinium source, a cerium source and a complexing agent are subjected to a sol-gel reaction, followed by calcination at a temperature above 1000°C (further 1100-1300°C) to obtain a ceramic substrate, which is then melt-compounded with a carbonate to obtain the ceramic substrate.
[0027] In the present invention, the temperature in the upgrading stage is 500 to 700°C, and further 550 to 650°C.
[0028] In the present invention, the atmosphere upgraded by the CO2 ceramic membrane is circulated to the anode chamber for recycling. In the present invention, the atmosphere upgraded by high temperature is directly recycled, which can not only improve the energy recovery efficiency, but also further improve the coupling efficiency of biomass gasification and SOFC power generation, and can further improve the yield of synthesis gas and the power generation energy density of SOFC.
[0029] The present invention also provides a device for implementing the shell-and-tube biomass carbon power cogeneration method coupled with CO2 membrane separation, comprising a tubular SOFC and a CO2 upgrading unit;
[0030] The tubular SOFC comprises an anode layer, an electrolyte layer composited on the surface of the anode layer, and a cathode layer composited on the surface of the electrolyte layer; the anode layer is arranged in a hollow tube shape, and the inner cavity of the hollow tube is the anode chamber;
[0031] The anode chamber is filled with biomass;
[0032] The tubular SOFC is provided with a gas inlet a for supplying gas to the anode chamber and an exhaust gas outlet for outputting exhaust gas; in addition, it also includes a gas inlet b for supplying gas to the surface of the cathode layer;
[0033] The CO2 upgrading unit separation container is separated by a CO2 ceramic membrane to form a permeation chamber and a retentate chamber; the permeation chamber is provided with a tail gas inlet, which is connected to the tubular SOFC tail gas outlet, and the retentate chamber is provided with an upgraded gas outlet;
[0034] Preferably, the upgraded gas outlet is connected to the gas inlet a of the tubular SOFC.
[0035] Beneficial Effects
[0036] The present invention innovatively gasifies biomass in situ in the inner cavity of the anode layer of the tubular SOFC and directly carries out SOFC power generation reaction with the anode layer, which can unexpectedly improve energy utilization, improve the coupling efficiency and effect of the two, significantly improve the preparation yield of synthesis gas, improve the power density of SOFC, and also help to achieve the selective application of high-temperature synthesis gas.
[0037] The method of the present invention can realize the energy cascade application, improve the efficient joint use of synthesis gas and SOFC, and furthermore, can realize the high-temperature selective quality improvement and application of high-temperature tail gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a flow chart of the biomass-based solid oxide fuel cell system coupled with CO2 separation of the present invention;
[0039] Figure 2 The composition and lower heating value distribution diagram of the gasified syngas at different temperatures of the B-SOFC unit;
[0040] Figure 3 This is a graph of gas flux at different CO2 concentrations and temperatures measured by permeation measurement;
[0041] Figure 4 This is a graph showing the operating voltage and power density of SOFC as a function of current density. DETAILED DESCRIPTION
[0042] The present invention provides an optional shell-and-tube biomass carbon-electricity cogeneration method coupled with CO2 membrane separation, comprising the following steps:
[0043] Step 1): Loading biomass solid particles
[0044] A certain mass of biomass is filled into the inner part of the sleeve SOFC tube (the inner cavity of the anode layer), and the sleeve SOFC is placed in a heating furnace to increase the temperature. At the same time, a certain flow of nitrogen is introduced as a protective gas, and all the gas in the device is exhausted and the air tightness is checked.
[0045] Step 2): Biomass gasification
[0046] After reaching the preset temperature, a certain flow of gas a (gasification gas, such as O2, H2O) is introduced into the casing. (g) Mixed gas), biomass undergoes gasification reaction to produce synthesis gas (gas b).
[0047] Step 3): In-situ power generation of gas b
[0048] The gas b synthesized in the SOFC cavity directly contacts the SOFC anode surface, the cathode surface sweeps over the air, an oxidation reaction occurs at the anode, electricity is generated in situ, and an anode tail gas (gas c) is produced.
[0049] Step 4): Separation and capture of CO2 in gas c
[0050] Gas c is introduced into a high-temperature permeation cell (containing a high-temperature ceramic carbonate two-phase membrane), and a certain flow of N2 is introduced into the permeation side as a sweep gas. CO2 is separated at 550°C to 650°C and enters the permeation side to improve the quality of the anode tail gas.
[0051] Step 5): Recycling of exhaust gas
[0052] The calorific value of the upgraded tail gas is increased and enters the retentate side, and is recycled to the aforementioned shell-and-tube SOFC, and the above process is repeated for recycling.
[0053] In the system described in the present invention, a membrane separation unit is matched with a B-SOFC unit that deeply couples biomass gasification and SOFC power generation, thereby achieving biomass resource utilization and efficient production of green electricity.
[0054] In the present invention, a microtubular solid oxide fuel cell (MT-SOFC) is selected, and its structure can be a tubular SOFC with an inner cavity as is well known in the industry, which can not only carry biomass solid particles, but also realize the direct in-situ power generation of the generated syngas, thus realizing the efficient power generation of SOFC for solid fuels. The MT-SOFC can adopt a three-layer structure of anode substrate-electrolyte-cathode. The thickness of the anode substrate can be controlled at 4.5-5.6mm, the thickness of the electrolyte layer and the cathode layer can be controlled at 80-120μm, and the anode can be Pt, Ag, LaNiO3, La 0.45 Sr 0.45 Ti 0.90 Ni 0.10 O 3-δ , NiO-YSZ, Ni-Ba CeO3 / BaZrO3, NiO-Gd 0.1 Ce 0.9 O 2-δ The electrolyte can be 8YSZ, Ce0.8 Sm 0.2 O 2-δ (SDC), Gd 0.1 Ce 0.9 O 2-δ (GDC), Ce 0.8 G 0.2 O 2-δ (CGO), (Bi 0.75 Y 0.25 ) 1.86 Ce 0.14 O 3±δ etc., the cathode material can be Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O 3-δ (BSCF), La 1-x Sr x CoO 3-δ (LSC), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ 、(La,Sr)MnO 3-δ 、LaSrCoO 4±δ , Mn 1.3 Co 1.3 Cu 0.4 O4, etc. During the treatment stage, the ventilation flow rate inside the tube is 5-20mL / min, the ventilation flow rate outside the tube is 50-200mL / min, and the working temperature is 700-750℃.
[0055] In the present invention, the biomass may be agricultural and forestry wastes such as wood chips and straw, or may be a series of organic solid wastes such as wet garbage or organic industrial garbage.
[0056] Preferably, the biomass is pine sawdust, and the mass fraction of moisture is 1% to 5%.
[0057] In the present invention, the gasifying agent may be one of oxygen-water vapor, air-water vapor and air.
[0058] Preferably, the gasifying agent is oxygen-water vapor.
[0059] In the present invention, biomass gasification is directly carried out at the tubular SOFC anode, together forming a B-SOFC unit, and the solid oxide fuel cell selects a hollow tubular cell (T-SOFC), which is composed of an anode layer, an electrolyte layer, and a cathode layer from the inside to the outside. The anode material can be Pt, NiO, etc., the electrolyte can be YSZ, GDC, etc., and the cathode material can be Pt, LSCF, LSM, etc.
[0060] As an optional solution, in the following cases, unless otherwise stated, the materials of SOFC are: anode material is NiO x -BaO-GDC, the electrolyte is GDC-10(Gd 0.1 Ce 0.9 O 2-δ ), the cathode material is LSCF (La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ ).
[0061] The electrode material and the battery can adopt conventional sleeve SOFC in the industry. In the present invention, as a feasible solution, they can be prepared by the following steps:
[0062] Step 1): Anode base tube forming
[0063] Gadolinium oxide doped cerium oxide and nickel oxide powder are mixed, anhydrous ethanol is added for wet ball milling and then dried to obtain mixture A, wherein the molar ratio of gadolinium oxide doped cerium oxide to nickel oxide is 2:3; pore-forming agent carbon black and binder PVB are added to mixture A and mixed to obtain mixture B, wherein the volume ratio of mixture A to powdered carbon black in mixture B is 2:1, and the volume ratio of mixture A to binder PVB in mixture B is 10:1; anhydrous ethanol is added to mixture B and fully mixed to obtain mixture C, wherein the volume ratio of mixture B to anhydrous ethanol is 1:9; mixture C is sent to a vacuum mud kneader for mixing and exhausting, and then microtubes are obtained by an extrusion molding method commonly used in industry, which is hung for air drying at room temperature for 12 hours, and then dried in a drying oven at 50-60°C for 12 hours to form an anode substrate precursor; the obtained precursor is pre-sintered at 1100°C for 5 hours to obtain an anode substrate.
[0064] Step 2): Electrolyte slurry preparation
[0065] Gadolinium oxide doped cerium oxide GDC-10 (Gd 0.1 Ce 0.9 O 2-δ ), adding binder PVB to the GDC-10 powder to obtain a mixture D, wherein the mass ratio of GDC-10 to PVB is 8:1; adding solvent pineneol to the mixture D and mixing thoroughly to obtain a mixture E, wherein the mass ratio of mixture D to pineneol is 1:1; using a vacuum pump at an absolute pressure of 200 mbar, degassing the mixture E.
[0066] Step 3) Cathode slurry preparation
[0067] Lanthanum strontium cobalt iron ferrite LSCF (La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ ), GDC-10 and LSCF were mixed, anhydrous ethanol was added for wet ball milling and then dried to obtain a mixture F, wherein the molar ratio of GDC-10 to LSCF was 2:3; a binder PVB was added to the mixture F to obtain a mixture D, wherein the mass ratio of GDC-10 to PVB was 8:1; a solvent pineneol was added to the mixture D and mixed thoroughly to obtain a mixture E, wherein the mass ratio of the mixture D to pineneol was 1:1; a vacuum pump was used to degas the mixture E at an absolute pressure of 200 mbar for 30 minutes.
[0068] Step 5): Electrolyte layer coating
[0069] One end of the pre-calcined NiO-GDC anode substrate tube was sealed with plastic wrap, and then immersed in the GDC electrolyte slurry. After standing for 15 seconds, it was slowly pulled up and dried. After repeating this process several times, it was calcined at 1350°C in a muffle furnace for 5 hours and polished to obtain a tubular half-cell with an electrolyte layer.
[0070] Step 6): Cathode layer coating
[0071] One end of the tubular half-cell with the electrolyte layer is closed, and then it is immersed in the cathode slurry, pulled and dried, calcined at 1300°C in a muffle furnace for 5 hours, and polished to obtain a microtubular solid oxide fuel cell (MT-SOFC) product.
[0072] Step 7): Battery Ba modification
[0073] Prepare a 0.1 mol / L Ba(NO3)2 solution, use a pipette to inject the solution into the battery, shake it slightly, let it air dry naturally, and repeat the process; place the battery in a muffle furnace and calcine it at 1200℃ for 2h to obtain a Ba-doped MT-SOFC modified battery.
[0074] Step 8): Battery wiring and assembly
[0075] Use a brush to evenly apply a layer of sintered silver paste on the surface of the battery, let it air-dry naturally, and then place it in a muffle furnace and calcine it at 750℃ for 3h; use 0.5mm diameter silver wire to wrap a silver grid, attach it to the surface of the silver paste, and then lead it out with a certain length of silver wire; grind a certain area on the outer surface of the battery until the anode surface is exposed, and then bond a 1cm long and 5mm wide current collector nickel felt to the area, and connect and lead it out with a silver wire with a ceramic insulating tube; use high-temperature sealant to connect two corundum ceramic tubes at both ends of the SOFC, install a quartz tube, and form a sleeve-type solid oxide fuel cell.
[0076] The operating temperature range of SOFC unit is 650℃-750℃.
[0077] In the present invention, an extrusion molding method is used to construct a T-SOFC anode substrate tube with an inner diameter of 4±0.5mm, a thickness of 1±0.2mm, and a length of 10-15cm. The electrolyte and cathode are coated by immersion pulling. The electrolyte layer is 50-100μm thick and the cathode layer is 100-200μm thick.
[0078] In the present invention, the anode tail gas can be subjected to subsequent carbon dioxide ceramic membrane upgrading treatment.
[0079] The carbon dioxide separation membrane can be a high-performance high-temperature ceramic carbonate dual-phase membrane, and the ceramic phase matrix can be La 1.5 Sr 0.5 NiO 4+δ ,La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ , Gd 0.2 Ce 0.8 O 2+δ Etc., the filling composite carbonate can be Li2CO3, Na2CO3 (52:48wt%) or Li2CO3, Na2CO3, K2CO3 (42.5:32.5:55wt%), etc.
[0080] In the present invention, the carbon dioxide separation membrane adopts a carbonate-filled ceramic biphasic membrane, including a ceramic matrix and a filling carbonate. The ceramic matrix material can be YSZ, GDC, etc., and the filling carbonate can be Li2CO3, Na2CO3, etc., carbonates with good thermal stability.
[0081] In the present invention, as an optional method, unless otherwise stated, the high-temperature ceramic carbonate dual-phase membrane (carbon dioxide upgraded ceramic membrane) used is prepared by the following steps:
[0082] Step 1): Gadolinium oxide doped cerium oxide GDC-20 (Gd 0.2 Ce 0.8 O 2+δ )
[0083] GDC-20 was prepared by EDTA-citric acid complexation method: gadolinium nitrate and cerium nitrate were dissolved in deionized water at a molar ratio of 1:4, and citric acid and ethylenediaminetetraacetic acid (EDTA) were added, and the molar ratio of total metal ions to citric acid and EDTA was 1:1:2; dilute ammonia water was added dropwise to adjust the solution pH to 8; the solution was transferred to a constant temperature magnetic stirrer, heated at 85°C for 6h, and the water was evaporated to obtain a viscous transparent gel; the gel was transferred to a vacuum drying oven and dried at 120°C for 10h to obtain a porous intermediate; the intermediate was placed in a muffle furnace and calcined at 1200°C for 5h to obtain the final GDC-20 finished powder.
[0084] Step 2): Disc-shaped ceramic matrix forming
[0085] Weigh 15g of homemade GDC-20 powder and spread it evenly into the disc mold. Use a laboratory infrared tablet press to pressurize it to 30MPa and maintain the pressure for 1h. Release the pressure and demold the molded disc with a diameter of 50mm and a thickness of 2.5mm. Put it into a muffle furnace and sinter it at 1500℃ for 6h to enhance the mechanical strength to obtain a disc-shaped ceramic matrix.
[0086] Step 3): Filling with composite carbonate
[0087] The carbonate filling was carried out by high-temperature melt impregnation method: 5 g of Li2CO3 and Na2CO3 with a mass ratio of 52:48 were weighed and mixed thoroughly in a mortar; the mixed carbonate was spread evenly on the surface of the ceramic substrate and placed in a muffle furnace and heated at 550°C for 5 hours to allow the carbonate to melt and impregnate into the pores of the ceramic phase; the substrate was taken out and inverted to the other side, and the above filling steps were repeated, followed by polishing to obtain a high-temperature ceramic carbonate two-phase membrane product.
[0088] The thickness of the separation membrane must ensure that the mechanical strength requirements are met under working conditions, for example, it can be 3-4 mm;
[0089] The operating temperature range of the separation membrane is relatively wide, which can be 500-700°C, meeting the margin for changes in anode tail gas temperature.
[0090] The present invention also provides a device for implementing the shell-and-tube biomass carbon power cogeneration method coupled with CO2 membrane separation, comprising a tubular SOFC and a CO2 upgrading unit;
[0091] The tubular SOFC comprises an anode layer, an electrolyte layer composited on the surface of the anode layer, and a cathode layer composited on the surface of the electrolyte layer; the anode layer is arranged in a hollow tube shape, and the inner cavity of the hollow tube is the anode chamber;
[0092] The anode chamber is filled with biomass;
[0093] The tubular SOFC is provided with a gas inlet a for supplying gas into the anode chamber and an exhaust gas outlet for outputting exhaust gas; in addition, it also includes a gas inlet b for supplying gas to the surface of the cathode layer;
[0094] The CO2 upgrading unit separation container is separated by a CO2 ceramic membrane to form a permeation chamber and a retentate chamber; the permeation chamber is provided with a tail gas inlet, which is connected to the tubular SOFC tail gas outlet, and the retentate chamber is provided with an upgraded gas outlet;
[0095] Preferably, the upgraded gas outlet is connected to the gas inlet a of the tubular SOFC.
[0096] In the following embodiments and comparative examples, the selected biomass is pine sawdust dried at 105°C under normal pressure for 24 hours, and it is assumed that the biomass completes gasification in 20 minutes; the gasification medium is oxygen, and its flow rate is 10% of the oxygen flow rate required for complete combustion of pine wood, and the ratio of water vapor to oxygen flow rate is 1:10; the permeation cell is wrapped with a layer of quartz insulation wool with an average thickness of 20 mm, the carbon capture rate is defined as the actual CO2 capture amount / the CO2 amount detected in the anode tail gas, and the energy utilization efficiency is defined as the unit biomass SOFC power generation / unit biomass calorific value.
[0097] The following are comparative examples and specific implementation methods:
[0098] Example 1
[0099] 1) Place 1g of biomass inside SOFC, pass 5ml / min of oxygen and 0.15ml / min of water vapor into the SOFC inlet to contact the biomass inside for gasification, and pass 20ml / min of air into the outside of the casing (in contact with the cathode surface). The gasification reaction is operated at 750℃ (marked as T, the operating temperature of the tubular SOFC, that is, the temperature of gasification and SOFC), and the lower calorific value of the syngas is 9.8MJ / m 3 The syngas yield per unit mass of biomass is 18.0mmol / g, the open circuit voltage is 0.913V, and the maximum power is 0.46W / cm 2 , the energy utilization efficiency is 59.63%;
[0100] 2) The anode tail gas is passed into the permeation cell, the average temperature of the retentate chamber is 670°C, the average temperature of the permeate chamber is 650°C, the tail gas on the retentate side is passed into the SOFC anode for recycling twice, and the CO2 capture rate is 68%.
[0101] Example 2
[0102] Compared with Example 1, the only difference is that the retentate side tail gas recirculation is not adopted.
[0103] 1) Place 1g of biomass inside SOFC, pass 5ml / min of oxygen and 0.15ml / min of water vapor into the SOFC inlet to contact and gasify the biomass inside, and pass 20ml / min of air into the outside of the casing. The gasification reaction is operated at 750℃, and the lower calorific value of the syngas is 9.7MJ / m 3 The syngas yield per unit mass of biomass is 17.8mmol / g, the open circuit voltage is 0.910V, and the maximum power is 0.28W / cm 2 , the energy utilization efficiency is 44.80%;
[0104] 2) The anode tail gas is passed into the permeation cell, the average temperature of the retentate chamber is 670°C, the average temperature of the permeation chamber is 650°C, and the CO2 capture rate is 43%.
[0105] Through Examples 1 and 2, the tail gas is upgraded at high temperature and then circulated, which can unexpectedly enhance the coupling efficiency of gasification and SOFC, further enhance the yield of synthesis gas, and not only that, but also help improve the maximum power.
[0106] Example 3
[0107] Compared with Example 1, the only difference is that the temperature T is changed. The experimental groups are:
[0108] Group A: temperature T is 700℃;
[0109] Group B: temperature T is 650℃;
[0110] Other operations and parameters are the same as in Example 1.
[0111] It can be seen from Examples 1 and 3 that optimizing and controlling the operating temperature of SOFC (the temperature of SOFC and gasification) can further enhance the coupling effect of the gasification and SOFC of the process described in the present invention, further improve the synthesis efficiency of the synthesis gas, and not only that, but also optimize the maximum power of SOFC.
[0112] Comparative Example 1
[0113] Compared with Example 2, the only difference is that the membrane separation unit is not activated.
[0114] 1g biomass was placed inside the SOFC, 5mL / min of oxygen and 0.15ml / min of water vapor were introduced into the SOFC inlet, and 20ml / min of air was introduced into the outside of the casing. The gasification reaction was operated at 750℃, and the lower calorific value of the syngas was 9.4MJ / m 3 The syngas yield per unit mass of biomass is 17.7mmol / g, the open circuit voltage is 0.907V, and the maximum power is 0.26W / cm 2 . The energy utilization efficiency is 21.46%.
[0115] Comparative Example 2
[0116] Compared with Example 2, the difference is that the biomass is not filled in the inner tube of the SOFC, and gasification is not carried out inside, that is, a fixed bed is used as the biomass gasification reaction site (the gasification conditions are the same as in Example 2), and the synthesis gas is transmitted by a pipeline wrapped with insulation cotton of equal quality and passed into the SOFC for power generation. The SOFC is placed in a heating furnace for insulation, and the power consumption of the heating furnace is subtracted from the power generation power of the SOFC when calculating the efficiency.
[0117] The results show that the lower calorific value of the syngas is 9.4MJ / m 3 The syngas yield per unit mass of biomass is 13.6mmol / g, the open circuit voltage is 0.906V, and the maximum power is 0.27W / cm 2 . The energy utilization efficiency is 36.78%;
[0118] The single-cycle CO2 capture rate is 41%.
[0119] Comparative Example 3
[0120] Compared with Comparative Example 2, the only difference is that the carbon dioxide in the tail gas is not upgraded and not recycled.
[0121] The results of the embodiments and comparative examples are shown in the following table.
[0122]
[0123] Figure 2 a and b specifically record the syngas distribution, gas production rate and lower heating value of the syngas at three system operating temperatures of Example 1 / 3 respectively.
[0124] Figure 3 a and b respectively record the CO2 capture performance at different CO2 tail gas concentrations and different permeation cell temperatures in Example 1 / 3.
[0125] Figure 4 The operating characteristic curves of SOFC at three temperatures in Example 1 / 3 are recorded.
[0126] It can be seen from the performance of the embodiment and the comparative example that under the same working conditions, tail gas recirculation significantly improves the utilization rate of biomass energy, and the energy utilization efficiency is significantly improved compared with the system without CO2 membrane separation and the system without biomass-SOFC coupling. The SOFC anode has a positive synergistic effect on the production of synthesis gas and the cracking of tar, and the synthesis gas yield is significantly improved compared with the catalysis without SOFC anode.
Claims
1. A coupled CO 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The biomass is pre-loaded in the anode chamber of the anode layer of the tubular SOFC, and then the tubular SOFC is heated to gasify the biomass in the anode chamber to form syngas and directly contact the anode layer to participate in SOFC power generation; the tail gas generated in the power generation stage is then converted into syngas through CO 2 Ceramic membrane quality improvement.
2. The coupled CO as claimed in claim 1 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The tubular SOFC comprises an anode layer arranged in a hollow tubular shape, an electrolyte layer compounded on the surface of the anode layer, and a cathode layer compounded on the surface of the electrolyte layer; the inner cavity of the hollow tubular is the anode chamber; Preferably, the inner diameter of the tubular SOFC is 5 to 30 mm, the thickness of the anode layer is 0.5 to 2 mm, the thickness of the electrolyte is 0.01 to 0.1 mm, and the thickness of the cathode layer is 0.01 to 0.1 mm.
3. The coupling CO as claimed in claim 2 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The materials of the anode layer include Pt, Ag, LaNiO 3 ,La 0.45 Sr 0.45 Ti 0.90 Ni 0.10 O 3-δ 、NiO-YSZ、Ni-Ba-CeO 3 / BaZrO 3 、NiO-Gd 0.1 Ce 0.9 O 2-δ At least one of; Preferably, the material of the electrolyte layer includes 8YSZ, Ce 0.8 Sm 0.2 O 2-δ (SDC), Gd 0.1 Ce 0.9 O 2-δ (GDC), Ce 0.8 G 0.2 O 2-δ (CGO), (Bi 0.75 Y 0.25 ) 1.86 Ce 0.14 O 3±δ At least one of; Preferably, the material of the cathode layer includes Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O 3-δ ,La 1-x Sr x CoO 3-δ ,La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ 、(La,Sr)MnO 3-δ 、LaSrCoO 4±δ , Mn 1.3 Co 1.3 Cu 0.4 O 4 One of them.
4. The coupled CO as claimed in claim 3 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The biomass includes at least one of agricultural and forestry waste, wet garbage, and industrial waste; Preferably, a gasifying agent is introduced into the anode chamber to gasify the biomass therein to form synthesis gas; Preferably, the gasifying agent includes at least one of air, oxygen, nitrogen and water vapor; Preferably, during the SOFC power generation stage, the synthesis gas formed in the anode chamber directly participates in the anode reaction with the anode layer medium, and the oxygen-containing atmosphere contacts the cathode surface to carry out the cathode reaction, thereby achieving SOFC power generation.
5. The coupling CO as claimed in claim 4 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The heating temperature of the tubular SOFC is 650-800°C, and the open circuit voltage in the power generation stage is 0.9-1.1V.
6. The coupled CO as claimed in claim 1 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that CO 2 The ceramic membrane includes a ceramic phase matrix and carbonate compounded therein; Preferably, the ceramic phase matrix comprises La 1.5 Sr 0.5 NiO 4+δ ,La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ , Gd 0.2 Ce 0.8 O 2+δ At least one of; Preferably, the carbonate comprises Li 2 CO 3 、Na 2 CO 3 , K 2 CO 3 At least one of; Preferably, the CO 2 The carbonate content in the ceramic membrane is 30-60%.
7. The coupled CO according to claim 6 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The CO 2 The ceramic membrane is prepared by the following steps: a gadolinium source, a cerium source and a complexing agent are subjected to a sol-gel reaction, and then calcined at a temperature above 1000°C to obtain a ceramic substrate, and then melt-compounded with a carbonate to obtain the ceramic substrate.
8. The coupled CO as claimed in claim 1 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that The temperature in the upgrading stage is 500-700°C, and further 550-650°C.
9. The coupled CO according to any one of claims 1, 6 to 8 2 Membrane separation shell-and-tube biomass carbon power cogeneration method, It is characterized in that CO 2 The atmosphere upgraded by the ceramic membrane is circulated to the anode chamber for recycling.
10. A method for implementing the coupling CO according to any one of claims 1 to 9 2 A membrane separation shell-and-tube biomass carbon power cogeneration method device, It is characterized in that Including tubular SOFC and CO 2 Quality improvement unit; The tubular SOFC comprises an anode layer, an electrolyte layer composited on the surface of the anode layer, and a cathode layer composited on the surface of the electrolyte layer; the anode layer is arranged in a hollow tube shape, and the inner cavity of the hollow tube is the anode chamber; The anode chamber is filled with biomass; The tubular SOFC is provided with a gas inlet a for supplying gas to the anode chamber and an exhaust gas outlet for outputting exhaust gas; in addition, it also includes a gas inlet b for supplying gas to the surface of the cathode layer; The CO 2 The upgrading unit separation container is provided with a CO 2 The ceramic membrane is separated to form a permeation chamber and a retentate chamber; the permeation chamber is provided with a tail gas inlet, which is connected to the tail gas outlet of the tubular SOFC, and the retentate chamber is provided with an upgraded gas outlet; Preferably, the upgraded gas outlet is connected to the gas inlet a of the tubular SOFC.
Citation Information
Cited By
Flue gas CO2 capturing system and method based on ceramic membrane separation technology